Silicone Sponge: Closed Cell, Open Cell and the Density That Decides

Compression force and compression set against density for closed cell and open cell silicone sponge
Closed cell sponge takes two and a half times the force of open cell at the same density, and sets about half as much.

Two materials that share a name

Silicone sponge is silicone rubber with gas in it. That is the only thing the two commercial types have in common. Closed cell sponge has discrete bubbles, each one sealed inside a wall of rubber, so the gas cannot escape and the material behaves like a collection of tiny balloons. Open cell sponge has a continuous network of voids connected to the surface, so air moves through it freely and the material behaves like a very soft, very springy foam.

The difference in behaviour is not a matter of degree. A closed cell sponge is nearly incompressible in the short term because the gas inside has to be compressed, and it recovers its shape when the load is removed. An open cell sponge is highly compressible because the air simply leaves, and it recovers because the rubber struts between the voids push back.

That single structural fact explains almost every application decision. Sealing, buoyancy and thermal insulation want closed cells, because a seal that leaks gas is not a seal. Cushioning, filtration, acoustic absorption and anything that has to breathe want open cells, because a cushion that cannot vent is a cushion that bottoms out.

プロパティ Closed cell Open cell
Cell structure Discrete sealed bubbles Interconnected voids open to the surface
Compression force at 25 percent 40 to 480 kPa, rising with density 15 to 190 kPa, rising with density
Compression set, 22 h at 150 °C 8 to 26 percent 12 to 38 percent
Air permeability Effectively zero High; the material breathes
Water absorption Very low High unless treated
Thermal conductivity 0.06 to 0.09 W/m·K 0.04 W/m·K and up, but convection dominates at thickness
Typical use Gaskets, seals, buoyancy, thermal breaks Cushions, acoustic liners, filters, pressure pads

Table 1 — The structural difference, and what follows from it.

How the cells are made

Closed cell silicone sponge is made by adding a chemical blowing agent to an HCR compound, usually azodicarbonamide, and moulding it in a press. The blowing agent decomposes at a temperature close to the cure temperature, which is the central difficulty of the process: the gas has to be released while the rubber is still soft enough to expand, but the rubber has to crosslink before the gas escapes.

In practice this is run as a two-stage process. The compound is given a short, partial cure in the press under just enough pressure to keep the blowing agent from acting, and then it is released or transferred to an oven where the expansion and the final cure happen together. Get the first stage wrong and the sponge is either unexpanded, because the rubber cured before the gas formed, or collapsed, because the gas formed before the rubber was strong enough to hold it.

Open cell sponge is usually made by mechanically frothing a silicone dispersion with air and then curing it, which leaves the bubble walls thin enough that they rupture and connect. Salt leaching is the other route: mix in a fine salt, cure, then wash the salt out, which leaves a very uniform open structure. Reticulation, burning the cell walls away with a flame or an oxidising atmosphere, converts a closed cell sponge into an open cell one and is used where a specific pore size is wanted.

Density is set by how much gas is generated and how much the rubber is allowed to expand, not by the mould cavity. Two sponges from the same tool can differ in density by 30 percent if the blowing agent loading or the press opening is different.

Density drives everything

Once the cell type is fixed, density is the variable that sets every mechanical property. A closed cell sponge at 0.20 g/cm³ is a soft, light, very compliant material that takes 40 kPa to compress 25 percent. At 0.80 g/cm³ the same chemistry takes 480 kPa, which is stiff enough to be used as a structural pad. That is a twelve-fold change in stiffness from a four-fold change in density, because stiffness in a foam scales faster than density does.

Compression set moves the other way in relative terms. It rises with density, because a denser sponge has more rubber carrying the strain and therefore more permanent deformation, but it rises slowly: from 8 percent at 0.20 g/cm³ to 26 percent at 0.80 in the closed cell case. The absolute numbers matter less than the comparison between the two structures. At every density, the open cell material sets about 1.4 times as much as the closed cell material.

Density, g/cm³ Closed cell force at 25%, kPa Open cell force at 25%, kPa Closed cell set, % Open cell set, %
0.20 40 15 8 12
0.30 80 30 10 15
0.40 140 55 13 19
0.50 210 85 16 24
0.60 300 120 20 30
0.80 480 190 26 38

Table 2 — Density against compression force and compression set, 22 hours at 150 °C.

There is a design rule hidden in that table. If a gasket needs a specific closure force, the way to get it is to choose the density, not to change the hardness of the base compound. Changing the base compound hardness changes the force by perhaps 20 percent across the full range of Shore A. Changing the density changes it by a factor of twelve. Density is the coarse control and compound hardness is the fine one, and getting that order right saves a lot of trial moulding.

Compression force and compression set are different questions

Compression force answers the question: how hard does this gasket push back? It is what you need to know to design a closure, a latch or a housing. Compression set answers a different question: after being squeezed at temperature for a long time, how much of the push-back is left? A gasket with good compression force and bad compression set seals perfectly on day one and leaks in month six.

Both are affected by density, but they are affected by different things as well. Compression force is mostly a function of density and cell structure. Compression set is mostly a function of the cure system and the post-cure, and only secondarily of density. A sponge that sets badly is usually under-cured, not too dense, and the fix is a longer post-cure rather than a formulation change.

This is why the two numbers should be specified together and why a supplier who quotes only one of them is telling you half a story. For a sealing application the useful pair is something like 150 kPa at 25 percent deflection and a set below 20 percent after 22 hours at 150 °C. For a cushioning application the set matters much less and the force curve matters much more.

A softer sponge always seals better. A softer sponge conforms better to a rough surface but it also takes set faster and it has less stored energy to recover. Very soft sponge is right for delicate closures and wrong for a flange that has to hold for a decade.

Moulding it, and the things that go wrong

Silicone sponge is almost always compression moulded, because the expansion has to be constrained by a tool. The tool is designed with a cavity that is smaller than the finished part, and the compound is loaded as a slight excess so that the cavity fills before the blowing agent acts. The press is then opened by a controlled amount, or the part is transferred, and the expansion happens against that gap.

  • Under-filling gives a short part with a dense skin and a porous core, because the compound did not have enough mass to fill the cavity before expanding.
  • Over-filling gives a part with a solid rim and a distorted shape, because the excess has nowhere to go and the flash land restricts it.
  • A cold tool gives a collapsed surface, because the skin cures before the gas arrives.
  • Too fast a press opening gives a coarse, uneven cell structure, because the gas expands faster than the rubber can accommodate it.
  • No post-cure gives high compression set and a smell that customers notice, because the decomposition by-products are still in the part.

The post-cure is not optional. Azodicarbonamide decomposition leaves residues, and those residues both smell and plasticise the rubber, which shows up as compression set. A staged post-cure from 150 to 200 °C over several hours drives them out. A sponge that smells of ammonia when the box is opened has not been post-cured properly, and it will also set badly.

Where each one is used

Closed cell sponge goes where a seal, a barrier or a buoyant body is needed. Gaskets for enclosures that have to meet an IP rating, thermal breaks between a hot part and a cold one, sealing rings in food and beverage equipment, buoyancy for marine and subsea hardware, and vibration isolation pads under sensitive equipment. In all of these the requirement is the same: the material has to keep gas where it is.

Open cell sponge goes where the material has to breathe, conform, or absorb. Cushioning for fragile parts in a case, acoustic lining inside a machine enclosure, pressure pads in a laminator or a printer, filtration and diffusion media, and medical padding where skin has to stay dry. The common thread is that air movement is a feature rather than a leak.

申し込み Cell type Density, g/cm³ なぜ
IP-rated enclosure gasket Closed 0.35 to 0.50 Water and dust cannot pass a sealed cell
Thermal break, 200 °C service Closed 0.40 to 0.60 Low conductivity and temperature resistance together
Subsea buoyancy Closed 0.25 to 0.35 Low density, and the cells survive pressure
Acoustic liner Open 0.20 to 0.30 Sound is absorbed in the connected voids
Cushion in a transit case Open 0.25 to 0.40 Air escapes, so the cushion does not bottom out
Medical padding Open 0.20 to 0.30 Breathable against skin

Table 3 — Application against cell type and density.

Specifying it so you get what you asked for

The most common purchasing failure in silicone sponge is a drawing that says "silicone sponge, 3 mm, soft" and nothing else. That description is compatible with a dozen different materials, and the one that arrives will be the one the supplier had in stock.

A usable specification has four elements. The cell type, closed or open. The density with a tolerance, typically plus or minus 10 percent. The compression force at a stated deflection, which is the property that decides whether the part works. And the compression set after a stated time and temperature, which is the property that decides whether it still works in a year.

If the part goes into a regulated application, add the standard callout. ASTM D1056 classifies flexible cellular materials by type and class, and a callout like 2A1 tells the supplier the cell type, the compression deflection range and the temperature resistance in three characters. It is worth the effort to learn the code, because it removes the ambiguity that a prose description leaves.

One last thing worth specifying: whether the sponge may be spliced. Large gaskets are often made as a ring from a spliced strip, and the splice is the weakest point and the place a leak starts. If a continuous moulded ring is required, say so, because the price difference is real and the supplier will quote the cheaper option if the drawing does not forbid it.

What is the difference between closed cell and open cell silicone sponge?

Closed cell has sealed bubbles, so it does not pass gas or water and it resists compression like a collection of balloons. Open cell has connected voids, so air moves through it and it compresses much more easily.

Which one is better for a gasket?

Closed cell, almost always. An open cell gasket passes water and air through the void network, so it cannot seal anything. Open cell is for cushioning and acoustic absorption.

How does density affect performance?

Stiffness scales faster than density: going from 0.20 to 0.80 g/cm³ raises the force at 25 percent deflection from 40 to 480 kPa. Compression set also rises, but much more slowly.

Why does my silicone sponge smell?

The blowing agent residues have not been driven out. A staged post-cure from 150 to 200 °C removes them, and it also fixes the compression set that the residues would otherwise cause.

Can silicone sponge be made in a closed mould?

It is made in a mould, but the mould has to open or the part has to be transferred so the material can expand. A fully closed cavity produces a solid part with no cells.

What is the maximum continuous temperature for silicone sponge?

Around 200 °C for a standard grade and 250 °C for a high-temperature grade, which is similar to solid silicone. The limitation is the cure system and the residual volatiles, not the cell structure.

Specifying a sponge gasket and not sure which density?

Send the closure force, the gap and the temperature. We will recommend a cell type and density, and tell you what compression set to expect after a year in service.

Talk to a silicone engineer

最新の投稿

WhatsApp
フェイスブック
ツイッター
LinkedIn
ピンタレスト
Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
jaJA

クイック見積もり

図面および詳細要件を下記までお送りください。

Emial: [email protected]

または下記のお問い合わせフォームにご記入ください: