Silicone Tube Extrusion: Cold Feed, Hot Cure and Tight Tolerance

Silicone tube extrusion line with a cold feed extruder feeding a hot air vulcanisation tunnel
Silicone goes through a machine that looks like a plastic extruder and behaves nothing like one. The barrel is cold and the curing happens downstream.

A thermoset through an extruder-shaped machine

Silicone tube is made on equipment that looks like a plastics line and is operated on completely different principles. The reason is that silicone rubber is a thermoset. It does not melt, it does not solidify by cooling, and it does not tolerate being held hot.

A thermoplastic extruder works by melting the polymer and pushing the melt through a die, then cooling it back to solid. A silicone extruder works by pushing a cold, already-compounded rubber through a die at a temperature low enough that nothing happens, and then curing it downstream in a separate oven. The barrel is water-cooled to around 20 to 30 °C. The screw is short and shallow. The compression ratio is close to 1.

Everything that follows from that inversion is what makes silicone tube a different trade from PVC or PE tube, and it is why a plastics extruder operator needs a different set of instincts to run one.

プロパティ Silicone rubber Thermoplastic (PVC, PE)
Behaviour on heating Cures, cannot be re-melted Melts, fully reversible
Barrel temperature 20 – 30 °C, water cooled 150 – 220 °C, heated
Screw L/D 10 – 15 : 1 25 – 35 : 1
Compression ratio 1.1 – 1.4 : 1 2.5 – 4 : 1
Where solidification happens Downstream oven, 200 – 250 °C Water tank, 10 – 20 °C
Scrap Cannot be re-melted; limited regrind use Fully recyclable
Dimensional control Cure shrinkage plus post-cure drift Cooling shrinkage only

Table 1 — Why a silicone line is not a plastics line. The screw geometry and the temperature direction are both reversed.

The compression ratio point deserves emphasis because it is counter-intuitive. A plastics screw compresses the material 3:1 along its length to generate shear heating and to compact the melt. A silicone screw is close to 1:1, because the compound is already fully mixed and because shear generates heat that will scorch it in the barrel. The screw's job is metering, not melting.

The two material forms, and which one makes tube

Form What it is How it is processed Used for tube?
HCR — high consistency rubber Gum-like sheet or strip, Mooney 30 – 80 Cold feed extruder, then oven cure Yes — the standard route
LSR — liquid silicone rubber Two-part liquid, 1000 – 5000 Pa·s Metered and mixed, injected or pumped Rarely — thin coating and moulding
RTV — room temperature vulcanising Paste in a cartridge Hand or dispensed, cures in air No — sealing and potting only
F-LSR / fluorosilicone LSR with fluorine, oil resistant As LSR Specialty, small bore

Table 2 — Silicone material forms. Extruded tube is almost always HCR, because it needs green strength to hold shape before curing.

The reason tube is made from HCR rather than LSR is green strength. An extruded tube has to hold its shape between the die and the oven, unsupported, for several seconds. HCR has enough body to do that. LSR is a liquid and would simply run, which is why LSR is used for moulded parts and coatings rather than for extrusion.

HCR arrives as a compounded strip or sheet, already containing catalyst, filler, pigment and any additives. It is fed into the extruder as a continuous strip, which is why the feed arrangement matters more than it does on a plastics line — an interruption in the strip is an interruption in the tube.

The line, from strip to spool

A silicone tube line has four stages that each have to be right, and the failure modes are different at each one.

Extrusion. A cold feed extruder with a water-cooled barrel and a short, shallow screw pushes the compound through a die. The die is where the tube's dimensions are set, and because the material is elastic rather than molten, die swell is large and predictable only by trial. A silicone die is typically cut 10 to 25% smaller than the target outside diameter to compensate.

Curing. The extrudate passes into a heated tunnel. This is where the tube becomes solid, and the tunnel type is chosen by wall thickness and production rate.

Cooling and haul-off. The cured tube is cooled and pulled by a haul-off. The haul-off speed relative to the extruder output sets the wall thickness and the diameter, so it is the main dimensional control on the line.

Post-cure. An optional but often required oven cycle that removes volatiles and completes the cure. It changes the mechanical properties and it changes the dimensions, which is why it belongs in the tolerance discussion.

パラメータ Typical setting なぜ
Barrel temperature 20 – 30 °C Keep the compound from scorching
Die temperature 40 – 70 °C Low enough to be safe, high enough for a smooth surface
スクリュー速度 10 – 40 rpm Low; shear heat is the enemy
ダイ・スウェル 10 – 25% of die opening Elastic recovery on exit, material dependent
Haul-off draw-down 1.0 – 1.6 : 1 Sets wall and diameter together
Tube concentricity Better than 10% of wall Die centring, checked at start-up

Table 3 — Extrusion settings for HCR silicone tube. The barrel being colder than the die is the inversion that catches plastics operators.

Die swell is larger and less predictable in silicone than in most thermoplastics because the compound is highly elastic and its relaxation is slow. A die that produces a 10 mm tube on one compound may produce 10.8 mm on another of the same hardness, and the only reliable approach is to cut the die slightly small and adjust, or to adjust the haul-off draw-down and accept a change in wall.

Curing: hot air, salt bath or continuous

The curing method is chosen by wall thickness. Heat has to reach the centre of the wall, and silicone is a poor conductor, so thick tube needs a medium that transfers heat better than air.

方法 ミディアム 温度 最適
Hot air vulcanisation (HAV) Air in a tunnel 200 – 260 °C Thin wall, under 3 mm; simple and clean
Salt bath (LCM) Molten salt eutectic 180 – 230 °C Thick wall; excellent heat transfer
Fluidised bed Hot glass beads 200 – 250 °C Thick wall, clean surface
Infrared Radiant heat High surface temperature Thin wall, fast line speeds
Steam (continuous) Pressurised steam 150 – 180 °C Where steam is available; needs a pressure tunnel

Table 4 — Continuous curing methods. Salt bath is the standard for thick wall because it conducts heat into the wall far faster than air.

Hot air is the cheapest and the most common, and its limitation is exactly what you would expect: air is a poor heat transfer medium, so the cure time for a 6 mm wall in an air tunnel is long enough that the tunnel has to be very long or the line has to run very slowly. A salt bath transfers heat an order of magnitude faster, and for tube above about 4 mm wall it is usually the only economic option.

The salt has to be washed off afterwards, which is a process step in itself and a source of complaints if it is done badly. Salt residue on a medical tube is a defect; the wash water has to be controlled and the rinse verified.

Cure temperature and time are set by the catalyst system, and the two systems behave very differently.

System Cure temperature By-product Post-cure Used for
Platinum addition 120 – 150 °C to initiate None Optional, improves properties Medical, food, transparent
Peroxide (dicumyl) 150 – 170 °C Acetophenone, methane Required, 200 °C for 4 h General industrial, thick sections
Peroxide (2,5-dimethyl) 160 – 180 °C Volatile fragments Required Where DCP volatility is a problem

Table 5 — Catalyst systems. Platinum leaves no by-product, which is why medical tube is platinum cured.

Platinum addition cure is a hydrosilylation reaction between vinyl groups and Si-H groups, and it produces no by-product at all. That is why platinum-cured silicone is the default for medical, pharmaceutical and food contact: there is nothing to extract. The trade-off is cost, sensitivity to catalyst poisons (sulphur, tin, some amines) and a shorter pot life once the two parts are mixed.

Peroxide cure generates volatile fragments that stay in the rubber until they are driven out. That is why a post-cure of 4 hours at 200 °C is standard: it is not completing the cure, it is removing the by-products. Skip it and the tube smells, tastes, and fails any volatiles test — and it also drifts dimensionally as the volatiles leave in service.

Tolerance, shrinkage and post-cure drift

Silicone tube tolerances are looser than thermoplastic tube, and the reason is that the material changes dimensions twice: once on cure and again on post-cure.

Dimension Under 10 mm 10 – 25 mm 25 – 50 mm
Inside diameter ±0.15 mm ±0.25 mm ±0.40 mm
Outside diameter ±0.15 mm ±0.30 mm ±0.50 mm
Wall thickness ±0.10 mm ±0.15 mm ±0.25 mm
Concentricity 10% of wall 10% of wall 12% of wall
Cut length ±0.5 mm ±1.0 mm ±1.5 mm

Table 6 — Practical tolerances for extruded silicone tube. Concentricity is the one that decides whether the tube seals.

Cure shrinkage for silicone is 2 to 4%, which is large, but it is mostly compensated by the die and by the draw-down. The problem is not the mean shrinkage, it is the variation: the same die and the same compound can give a 0.3 mm spread in outside diameter across a shift, because cure temperature, haul-off tension and compound viscosity all move.

Post-cure adds a second, smaller shift. A tube that measures 10.00 mm off the line will measure about 9.95 mm after a 4 hour post-cure, and the change is not perfectly uniform along the length. This is why a tube measured before post-cure is not the tube the customer receives, and why the tolerance has to be applied to the finished, post-cured part.

Measure after post-cure. A dimension taken off the line is an intermediate value. If the part gets a post-cure, the tolerance applies to what comes out of the oven, not what goes in.

Defects, and what causes them

欠陥 原因 Fix
Rough or matt surface Die too cold, or compound too stiff Raise die temperature 5 – 10 °C
Bubbles or voids in the wall Air entrained in the compound, or moisture Vacuum-strip the feed, re-mill the compound
Under-cure, tacky surface Tunnel too short or too cool for the line speed Slow the line, raise the temperature, or both
Over-cure, hard and brittle Too much heat or too long in the tunnel Reduce temperature or increase line speed
Eccentric wall Die off-centre, or a mandrel that has drifted Re-centre the die, check the crosshead
Diameter drift along the length Haul-off tension varying, or feed interruption Check the haul-off and the strip feed
White bloom on the surface Peroxide by-products not driven off Post-cure properly
Split along the length Die line, or too much draw-down Reduce draw, polish the die land
Poor tear strength Under-cure, or wrong catalyst level Check cure, check compound

Table 7 — Silicone tube defects. The bloom row is a post-cure failure that looks like a material failure.

Bubbles are the defect that most often gets misattributed. Silicone compound is mixed on a two-roll mill and it entrains air; the standard fix is to vacuum-strip the compound before it is formed into strip, and to feed the extruder under a slight vacuum at the throat. If bubbles appear only in thick sections, the cause is more likely trapped air that could not escape before the skin cured, which points at cure temperature rather than at mixing.

Die lines are the other common one, and they are a tooling issue rather than a process one. A scratch or a carbon deposit on the die land leaves a continuous longitudinal mark, and no amount of temperature or speed adjustment removes it. Polish the land.

Grades, certification and what to ask for

Silicone tube is bought against a certification as often as against a dimension, and the certification is what separates a commodity tube from a medical one.

Requirement What it covers Ask for
FDA 21 CFR 177.2600 Rubber articles for repeated food contact Compound statement of compliance
USP Class VI Biological reactivity, implant-adjacent Test report per batch
ISO 10993 Biocompatibility, part 5 cytotoxicity and others Full test package, not a claim
BfR XV German food contact recommendation Compound certificate
REACH / RoHS Restricted substances Declaration per batch
Platinum cure No peroxide by-products Stated on the certificate, not implied
Post-cured Volatiles removed Cycle record, temperature and time

Table 8 — Certifications for silicone tube. The last two rows are process claims that are often asserted and rarely documented.

"Platinum cured" and "post-cured" are the two claims most often made without evidence. Both are process facts that should appear on a certificate of analysis with a temperature and a time, and both change what the tube can be used for. A tube that is platinum cured but not post-cured will pass a cytotoxicity test and fail a volatiles test, and the difference only shows up when the customer runs their own validation.

Hardness is the other specification worth pinning down. Silicone tube is normally supplied between Shore A 40 and 70, and hardness affects everything: a 40 Shore A tube is soft and seals on low force, a 70 Shore A tube resists collapse under vacuum. Specifying "silicone tube" without a hardness is leaving the most important property to the supplier.

Can silicone tube be made on a normal plastic extruder?

Not sensibly. A plastics screw has a 3:1 compression ratio and a heated barrel, both of which will scorch silicone compound in the barrel. Silicone needs a short, shallow, water-cooled screw with a compression ratio close to 1.

Why is the barrel cold and the die hot?

The compound must not cure in the barrel, so the barrel is water-cooled to 20–30 °C. The die is warmer, 40–70 °C, so the extrudate has a smooth surface and enough flow to form. All the curing happens in the tunnel downstream.

How is silicone tube cured?

Continuously, in a hot air tunnel at 200–260 °C for thin wall, or a molten salt bath at 180–230 °C for thick wall. Salt conducts heat far better, which is why it is used above about 4 mm wall.

Why does my silicone tube smell?

Peroxide cure by-products that were not driven off. A 4 hour post-cure at 200 °C removes them. Platinum-cured tube has no by-products and does not have this problem.

What tolerance can extruded silicone tube hold?

About ±0.15 mm on diameter under 10 mm, ±0.30 mm from 10 to 25 mm, and ±0.50 mm above 25 mm. Concentricity of 10% of wall is the practical limit and it matters more than diameter for sealing.

Why does the diameter change after post-curing?

Post-cure drives off volatiles and completes the cure, and the part shrinks slightly as it does — around 0.05 mm on a 10 mm tube. Tolerance has to be applied to the post-cured part, not to the dimension off the line.

What is the difference between platinum and peroxide cure?

Platinum addition cure produces no by-products and is the default for medical and food contact. Peroxide cure produces volatile fragments that require a long post-cure, but it is cheaper and more tolerant of compound contamination.

Can silicone tube be sterilised repeatedly?

Yes, which is a major reason it is used in medical and pharmaceutical tubing. It withstands autoclave cycles at 121–134 °C, gamma irradiation and ethylene oxide. Repeated autoclaving does gradually reduce tear strength.

Need silicone tube to a medical or food-contact specification?

Tell us the ID, wall, hardness, cure system and the certification you have to meet. We will confirm whether the tolerance is achievable and what the post-cure and documentation package looks like.

Talk to a tube extrusion engineer

最新の投稿

WhatsApp
フェイスブック
ツイッター
LinkedIn
ピンタレスト
Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
jaJA

クイック見積もり

図面および詳細要件を下記までお送りください。

Emial: [email protected]

または下記のお問い合わせフォームにご記入ください: