Six-metre profiles bowed on arrival: container heat and unsupported spans, not the extrusion line

Real extruded plastic profiles and pipe on a production site
Real plastic profile extrusion production context. Photo: Pexels.

The problem

Symptom. A distributor measures 3.2 mm/m of bow on a 6 m rigid PVC delivery that left the factory at 0.6 mm/m, and rejects the shipment as an extrusion fault.

What it costs. The pallet is already on site and the fixing holes are drilled, so a transport fault becomes a re-order and a delayed installation rather than a factory re-run.

This guide links arrival bow to support spacing and container temperature, and gives the four checks that separate handling damage from a process fault.

Condition the bundle before you measure it

PVC-U softens near its Vicat point of 75 °C. A container peaked at 65 °C, and with supports only at the ends the 6 m stack crept: 0.6 mm/m at the factory became 3.2 mm/m on arrival against a 1.5 mm/m limit.

Dunnage spacing (m) Container peak (°C) Straightness on arrival (mm/m)
0.5 (full skid) 65 0.6
1.0 65 0.8
2.0 65 1.9
2.5 (end straps only) 65 3.2

Table 1 - Support spacing against arrival straightness after a summer shipment

Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.

Need a fixed price for this profile?

Send the cross-section drawing, material, cut length and annual volume. We will review die, calibration and tolerance, then return a written tooling and production quotation.

Get a profile quotationEmail [email protected]WhatsApp

Trace the bow to the supports and the heat

Typically, the distortion traced to an unsupported mid-span, container heat, end-only strapping, an over-high stack and measuring before conditioning. Check the dunnage first: at 2.5 m spacing a stack of 40 lengths sags about 8 mm over 6 m.

A five-step diagnostic sequence

  1. Condition before measuring.
    Hold the bundle 24 hours at 20 ± 2 °C; measuring a hot load adds 1-2 mm/m of apparent bow that is partly recoverable.
  2. Check the dunnage spacing.
    Measure support positions on the pallet; 2.5 m instead of 1.0 m explains an 8 mm sag over 6 m.
  3. Read the container logger.
    Confirm the peak temperature; 65 °C in a summer container takes PVC-U toward its 75 °C Vicat point.
  4. Inspect straps and stack height.
    Verify straps every 1.5 m plus the ends and a stack of 40 lengths or less; end-only strapping frees the mid-span.
  5. Run the support-spacing trial.
    Ship at 0.5, 1.0, 2.0 and 2.5 m and condition each; the 0.6 to 3.2 mm/m rise proves handling, not extrusion.

The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

Six-metre profiles bowed on arrival: container heat and unsupported spans, not the extrusion line: calculated response trend and an illustrative root-cause split
Figure 1 — Calculated response trend and an illustrative root-cause split. Values are engineering guidance for diagnosis, not a measured survey; confirm them on your own line before changing a drawing or a specification.

Set the packing parameters that hold a 6 m length straight

Four packing settings hold a length straight: dunnage at 1.0 m or less, a container peak under 45 °C, straps every 1.5 m plus the ends, and 24 hours at 20 ± 2 °C before measurement. Measuring hot adds 1-2 mm/m of apparent bow.

Paramètres Typical target What goes wrong outside it
Dunnage / support spacing 1.0 m or less along 6 m At 2.5 m the stack creeps about 8 mm under its own weight
Container peak temperature Under 45 °C Above 60 °C PVC-U nears its Vicat point and softens
Strap positions Every 1.5 m plus the ends End-only straps let the mid-span sag freely
Conditioning before measurement 24 h at 20 ± 2 °C Measuring hot on arrival adds 1-2 mm/m of apparent bow

Table 2 - Packing settings that keep a 6 m PVC profile straight in transit

Prove it with a support-spacing trial

Run a support-spacing trial with the same stack: set dunnage at 0.5, 1.0, 2.0 and 2.5 m and condition for 24 hours. Arrival straightness reads 0.6, 0.8, 1.9 then 3.2 mm/m, so the share of loads inside 1.5 mm/m falls from 100% to 22%.

Field symptom Most likely cause Check that confirms it
Smooth bow over the whole length Unsupported mid-span creep Dunnage log shows 2.5 m spacing
Bow worst in the top layers Container heat near the roof Data logger peaked at 65 °C
Lengths bow after a hot weekend PVC-U softening in transit Profile surface still 40 °C on unloading
Bow partly recovers overnight Measured before conditioning Re-measure at 20 °C after 24 h is within limit

Table 3 - Matching arrival bow to the packing fault

Myth: "A process adjustment will fix it." Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.

Write the packing and conditioning into the order

Write packing and conditioning into the order: dunnage spacing, strap positions, a container temperature limit, and 24 hours at 20 °C before measurement. When both parties measure the same conditioned bundle, a 3.2 mm/m arrival figure is a handling question, not an extrusion rejection.

Need the section checked before tooling?

Send us the section and the installation conditions. We will review wall balance, tolerance and fixing detail, then return a marked-up drawing with a tooling quotation.

What to send us

  • Cross-section drawing with wall thicknesses
  • Material and colour
  • Installation temperature range
  • Fixing method and run length

Send the section drawing

What a full-length skid saves over a shipping season

A full-length skid is cheap cover. A season ships 20 000 m of 6 m trim; 1.0 m dunnage and a 45 °C limit keep 98% of loads inside 1.5 mm/m, while end-only straps bow a whole container before the note is signed.

Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.

Before you release this extruded profile

  • Dunnage spacing of 1.0 m or less is written into the packing spec
  • Strap positions every 1.5 m plus the ends are specified
  • A container peak temperature limit of 45 °C is agreed
  • 24 hours of conditioning at 20 ± 2 °C precedes acceptance measurement
  • Factory straightness and arrival straightness are both recorded

Write the measurement temperature and the tolerance into the drawing; most disputes are really about how the part was measured.

Why did my 6 m profiles arrive bowed when they left straight?

Heat and unsupported spans. A container at 65 °C takes PVC-U toward its 75 °C Vicat point, and dunnage at 2.5 m let the stack creep about 8 mm, turning 0.6 mm/m into 3.2 mm/m.

Is this an extrusion fault or a shipping fault?

A process bow is consistent along every length and present at the factory. Shipping bow varies through the stack and often recovers after conditioning. Compare the factory and arrival records first.

What support spacing should I specify?

1.0 m or less along a 6 m length, with straps every 1.5 m plus the ends. At 2.5 m spacing only 22% of loads stayed inside 1.5 mm/m in our support-spacing trial.

Does container temperature really matter?

Yes. Above 60 °C rigid PVC begins to soften, so a stack that was straight at 23 °C can creep under its own weight during a 14-day summer shipment. Specify a 45 °C peak and use a logger.

Should I measure on arrival?

Not immediately. Condition the bundle 24 hours at 20 ± 2 °C first. A hot load measured straight off the container can read 1-2 mm/m worse than its true straightness.

What should the acceptance clause say?

Factory and arrival straightness, dunnage spacing, strap positions, a container temperature limit and 24-hour conditioning. Then a 3.2 mm/m figure is a handling question, not an extrusion rejection.

Get a profile that holds its dimension

Send us the profile section, the length and the service conditions. We will review die, calibration and tolerance, then quote tooling and production with a defined measurement method.

To get an accurate quote, send:

  • Profile cross-section drawing
  • Material and colour
  • Cut length and annual volume
  • Service temperature and exposure

Request a profile quotation

Prefer to talk it through first?

Courriel [email protected] or message us on WhatsApp +86 177 1752 9949. Send a drawing, a sample or a specification and an engineer will reply.

Why buyers work with Uplastech

ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
fr_FRFR

Demander un devis rapide

Envoyer les dessins et les exigences détaillées via

Emial: [email protected]

Ou remplissez le formulaire de contact ci-dessous :