Nylon (PA6 / PA66) Injection Molding: Moisture, Conditioning and Dimensions

Black glass-filled nylon injection moulded gears and a natural nylon bush on a metrology bench with a micrometer
Glass-filled PA66 gears and an unfilled natural nylon bush. The gears hold tolerance because the glass restrains moisture uptake; the natural bush will grow 0.3 mm over a season and is measured wet, not dry.

The material that changes size after it leaves you

Polyamide — nylon 6 and nylon 66 — is the workhorse engineering plastic for anything that needs toughness, wear resistance, temperature resistance and resistance to oils and fuels. Gears, bushes, cable ties, connectors, under-bonnet parts, power-tool housings and conveyor components are all nylon.

It also has a property that causes more quality disputes than any other in injection moulding: it absorbs water and grows. A dry PA66 part left in a normal room reaches equilibrium at 1.5 – 2.5 % moisture and grows by 0.3 – 0.6 % in every dimension. That is 0.3 mm on a 50 mm part. If the drawing does not say whether the tolerance applies to the dry part or the conditioned part, the drawing is incomplete.

The number to design around: unmodified PA66 grows 0.3 – 0.6 % between the dry-as-moulded state and equilibrium at 23 °C / 50 % RH. Glass-filled grades grow 0.1 – 0.2 %. This is not shrinkage — that happens in the tool — it is moisture uptake in service, and it continues for weeks after moulding.

Grades

Grade Key property Moisture uptake at equilibrium Used for
PA6 unfilled Tough, good surface, cheaper 2.5 – 3.0 % Bushes, general parts
PA66 unfilled Higher strength and HDT than PA6 1.5 – 2.5 % Gears, structural parts
PA6 / PA66, 30 % GF Modulus 9 – 10 GPa, HDT 200 °C+ 0.8 – 1.5 % Brackets, housings, fans
PA66, 30 – 35 % GF, heat stabilised Continuous 150 °C 0.8 – 1.2 % Under-bonnet
PA6, impact modified Notched Izod 80 – 120 J/m 2.0 – 2.8 % Power tools, sports goods
PA66, mineral filled Low warp, good surface 1.2 – 1.8 % Automotive exterior
PA12 / PA11 Lowest moisture uptake, flexible 0.8 – 1.2 % Fuel lines, precision parts
PA6/6T, PPA High temperature, low moisture 0.3 – 0.6 % Lead-free solder reflow, automotive
Cast PA (MC nylon) Very high molecular weight 2.0 – 2.8 % Large bushes, sheets — not moulded

Table 1 — Polyamide grades. PA12 and PPA exist mainly to solve the moisture problem.

Moisture: drying, then re-absorbing

There are two completely separate moisture issues with nylon, and confusing them is the root of most problems.

Issue When Target Consequence if wrong
Too wet at the hopper Before moulding < 0.1 % (PA6), < 0.08 % (PA66) Hydrolysis: molecular weight drop, brittle parts, silver streaks
Too dry in service After moulding Conditioned to 1.5 – 2.5 % Part grows, but also becomes tougher — dry nylon is brittle

Table 2 — The two moisture problems. They have opposite targets.

Drying method PA6 PA66 PA66-GF30
Desiccant dryer, 80 °C 4 – 6 h 4 – 6 h 3 – 4 h
Desiccant dryer, 100 °C 2 – 3 h 2 – 3 h 2 h
Vacuum dryer, 90 °C 1.5 – 2 h 1.5 – 2 h 1 – 1.5 h
Hot air oven, 90 °C 6 – 8 h 6 – 8 h 4 – 6 h
Dew point requirement −20 °C −20 °C −20 °C

Table 3 — Drying schedules. Over-drying above 110 °C oxidises nylon and yellows it.

Note the second row of Table 2: dry nylon is brittle. A freshly moulded, bone-dry PA66 part will snap where the same part conditioned for two weeks will bend. This is why nylon parts are often conditioned deliberately — either by leaving them in a humid chamber, or by boiling them in water for 30 – 60 minutes, which accelerates uptake to near-equilibrium in an hour.

Conditioning method Time to equilibrium 참고
Ambient, 23 °C / 50 % RH 2 – 6 weeks (depends on wall) Uncontrolled; not a process
Humidity chamber, 70 % RH 1 – 2 weeks Controllable and repeatable
Hot water, 80 – 100 °C 1 – 4 h Fast; can relieve stress too
Steam autoclave 1 – 2 h Fastest; risk of over-absorption

Table 4 — Conditioning routes. Hot water is the practical answer for production.

Myth: "the part measured 50.00 mm, so it's in tolerance." If it was measured an hour after moulding, it was still dry. Three weeks later it measures 50.25 mm and the customer rejects it. Every nylon drawing must specify the conditioning state — dry as moulded, or conditioned to 23 °C / 50 % RH — and the two give different nominal dimensions.

Processing window

매개변수 PA6 PA66 PA66-GF30
용융 온도 230 – 260 °C 270 – 295 °C 280 – 300 °C
Barrel profile 220 / 235 / 245 / 250 °C 250 / 270 / 285 / 290 °C 260 / 280 / 295 / 295 °C
Mould temperature 60 – 90 °C 70 – 100 °C 80 – 100 °C
Injection pressure 70 – 110 MPa 80 – 130 MPa 90 – 150 MPa
Injection speed 빠른 빠른 Moderate — fibre breakage
Hold pressure 50 – 70 % of injection 50 – 70 % 60 – 80 %
Back pressure 0.5 – 1.0 MPa 0.5 – 1.0 MPa 0.3 – 0.8 MPa
Residence time < 8 min < 6 min < 6 min
수축 1.2 – 2.0 % 1.0 – 2.0 % 0.2 – 0.5 %
Regrind Up to 25 % Up to 25 % Up to 15 % (fibre shortening)

Table 5 — Processing windows. PA66 needs roughly 35 °C more melt temperature than PA6 for the same viscosity.

Mould temperature is the lever that controls crystallinity, and therefore strength, wear resistance and dimensional stability. A PA66 part moulded at 40 °C has a thin amorphous skin, low crystallinity in the core, and poor wear resistance; the same part at 90 °C is fully crystalline and performs as the datasheet says. For gears and wear parts, a hot mould is not optional.

Design rules

기능 Rule Why nylon is different
Wall thickness 1.0 – 3.5 mm Thick walls have a moisture gradient for months
Wall uniformity Within 15 % Differential moisture uptake causes warpage after moulding
Draft 0.5 – 1° Nylon releases well and is slippery
Ribs 0.5 × wall Thicker ribs hold moisture differently and swell
Bosses Wall 0.6 × nominal Boss cores stay hot; voids form
Gate Large; avoid restrictive gates on GF grades High shear degrades melt and breaks fibres
Tolerance Do not specify below ±0.1 mm on unfilled PA Moisture movement exceeds the tolerance
Metal inserts Design for 1 % differential growth Nylon grows; metal does not — inserts can split the boss
Sharp corners Internal R ≥ 0.5 × wall Nylon is notch sensitive when dry

Table 6 — Nylon design rules. The tolerance row is the one that causes the most arguments.

Gears and wear parts

Nylon is the default material for moulded gears and bushes, and the reasons are specific: it has a low coefficient of friction, it tolerates shock loads, it runs without external lubrication in many applications, and it damps noise.

Requirement Grade Design note
Low load, quiet running PA66 unfilled Cheapest; swells most
Higher torque PA66 + 30 % GF Stronger but more abrasive to the mating gear
Mating pair PA66 gear + POM pinion Dissimilar materials reduce wear and noise
High speed PA46 or PPA Better heat resistance at the tooth flank
Wet environment PA66 + GF, or POM POM absorbs less water and holds tolerance better
Food contact PA66 natural, food grade Check the colourant

Table 7 — Gear material selection. Never run nylon against nylon in a loaded pair — it welds and tears.

Gear tolerances need a note: a moulded nylon gear is normally specified to AGMA 8 – 9 or DIN 9 – 10, not to the precision of a machined gear. If the application needs better, the gear is machined from cast nylon or from POM.

Defects and causes

결함 원인 Fix
Brittle parts Over-dried, over-heated, or too much regrind Check moisture (not too low), melt temperature and regrind ratio
Silver streaks Moisture above 0.15 % Dry longer or hotter; check dew point
Bubbles in thick sections Moisture, or voids from shrinkage Dry; increase hold pressure and time
Warpage weeks after moulding Differential moisture uptake from uneven walls Uniform walls; condition before inspection
Dimensions drifting in service Moisture uptake Specify conditioned dimensions; use GF grade or PA12
Flash Low viscosity at high melt temperature Lower melt; check clamp tonnage
Short shots on GF grades High viscosity, cold mould Raise melt and mould temperature; enlarge gates
Yellow / brown parts Over-heating or long residence Lower melt 10 °C; reduce barrel residence
Cracks around inserts Insert expansion plus dry, brittle nylon Condition the part; increase boss wall; pre-heat inserts

Table 8 — Nylon defects. "Brittle" and "wet" can both be true at once — they are different faults.

The moisture gradient: why thick parts keep moving

Moisture enters nylon from the surface. On a 1 mm wall, equilibrium is reached in a few weeks and the whole section moves together. On a 5 mm wall, the outside reaches equilibrium in weeks while the core is still dry, and the part continues to change shape for months.

Wall thickness Time to 90 % of equilibrium at 23 °C / 50 % RH Time at 70 % RH
1 mm 2 – 3 weeks 1 – 2 weeks
2 mm 5 – 8 weeks 3 – 5 weeks
3 mm 10 – 16 weeks 6 – 10 weeks
5 mm 6 – 10 months 3 – 5 months
8 mm 18 – 30 months 10 – 18 months

Table 9 — Moisture diffusion times for unfilled PA66. Thick sections are never in equilibrium in service.

The engineering consequence is that a thick nylon part should be designed as a dry part with generous tolerances, or made from a glass-filled grade, or made from PA12. Specifying ±0.05 mm on a 5 mm thick unfilled PA66 part is not achievable in any state, because the part is a different size in every month of its first year.

The practical rule: if the wall is under 2 mm and the drawing specifies the conditioning state, unfilled PA is workable. If the wall is over 3 mm, or the tolerance is tighter than ±0.1 mm, move to a glass-filled grade. Above 5 mm, move to PA12 or accept that the tolerance applies only at one defined moisture content.

Glass fibre: what you gain and what you lose

속성 PA66 unfilled PA66 + 30 % GF Change
Tensile strength 80 MPa 185 MPa +130 %
Flexural modulus 2.8 GPa 9.5 GPa +240 %
HDT at 1.82 MPa 75 °C 250 °C +175 °C
Elongation at break 25 – 60 % 2 – 3 % −90 %
Notched Izod 50 – 70 J/m 70 – 95 J/m +40 %
Moisture growth in service 0.3 – 0.6 % 0.1 – 0.2 % −65 %
수축 1.2 – 2.0 % 0.2 – 0.5 % −75 %
뒤틀림 Low–moderate High (anisotropic) Worse
Abrasion of the tool 낮음 높음 Requires hardened steel
Weld line strength 70 – 90 % of parent 40 – 60 % of parent Much worse

Table 10 — The cost of glass. Stiffness and stability go up; elongation, weld strength and tool life go down.

The weld-line row is the one that fails parts in the field. In a glass-filled material, the fibres do not cross the weld — they lie parallel to the weld line, so there is a plane of unreinforced resin across the part. A 30 % GF nylon part with a weld line in a loaded location behaves like an unfilled part there, and often worse, because the fibres create a notch. If a weld line cannot be avoided, move it out of the load path or use a mineral-filled grade where the filler is more isotropic.

Under-bonnet: the real requirements

Condition Test Grade requirement
Continuous heat 1,000 h at 120 – 150 °C Heat-stabilised PA66, or PA66/PPA
Peak heat 1,000 h at 150 – 180 °C PA66/6T, PPA, or PA46
Thermal cycling −40 to +150 °C, 1,000 cycles Heat-stabilised, impact modified
Hot air ageing 1,000 h at 150 °C, property retention > 50 % Heat-stabilised grade only
Coolant contact Glycol at 100 °C Hydrolysis-stabilised
Fuel contact Petrol, diesel, ethanol blends PA12 or a fuel-resistant grade
Salt spray 500 h Not a nylon property — protect the inserts

Table 11 — Under-bonnet requirements. The heat-stabiliser package is what separates an automotive grade from a general-purpose one.

Heat stabilisation is a real additive package, not marketing. Unstabilised PA66 loses about 70 % of its tensile strength after 1,000 hours at 150 °C; a properly stabilised grade loses 20 – 30 %. The difference is a copper or organic stabiliser system that interrupts the thermal oxidation chain. It costs 10 – 20 % more per kilogram and it is not optional for anything that lives near an engine.

Frequently asked questions

Should I specify PA6 or PA66?

PA66 for higher strength, stiffness and heat resistance; PA6 for toughness, surface finish and cost. PA6 also processes 30 – 40 °C cooler, which matters if your machine is limited. For most general parts the difference is small; for under-bonnet or high-temperature work, PA66 or a high-heat grade.

Why do my nylon parts measure differently a month later?

Moisture uptake. Dry nylon grows 0.3 – 0.6 % as it absorbs water to equilibrium. Either specify and inspect in the conditioned state, or switch to a glass-filled grade where the growth is 0.1 – 0.2 %, or to PA12/PPA where it is lower still.

Can I boil nylon parts to condition them?

Yes — 30 – 60 minutes in water at 80 – 100 °C brings most parts close to equilibrium and also relieves moulding stress. It is a standard production step for nylon gears and bushes. Do not boil glass-filled parts for long periods; the sizing on the fibre can be affected.

How much regrind can I use?

Up to 25 % on unfilled grades, 15 % on glass-filled (the fibres shorten with each pass). Regrind must be dried again, and it must be the same grade and colour. Do not use regrind in parts that will be conditioned and held to tolerance.

What is the difference between PA6 and PA6/6T?

PA6/6T is a semi-aromatic polyamide with a much higher melting point (around 325 °C) and much lower moisture uptake. It is used where the part must survive lead-free solder reflow (260 °C) or hold tolerance in humid conditions. It costs 3 – 5× PA66 and needs a hot-runner system rated for 340 °C.

Why is my glass-filled nylon part warping?

Fibre orientation. Glass fibres align with the flow and restrain shrinkage strongly in that direction and weakly across it, so a part with a long flow path warps. Fixes: gate from the centre, use a mineral/glass hybrid filler, raise mould temperature, or redesign the wall to be more uniform.

Does nylon need a hot runner?

Not necessarily, but it benefits more than most materials. Nylon's high melt temperature and narrow processing window mean a cold runner wastes a lot of material and creates a lot of regrind. On a 16-cavity tool the runner can be 60 % of the shot.

Is nylon UV stable?

No. Unstabilised nylon yellows and embrittles outdoors within a year. UV-stabilised grades extend this to 3 – 5 years, and carbon-black-filled grades do better. For long outdoor life, use a painted or coated part, or a different material.

Moulding a nylon part and fighting tolerance drift?

Send the drawing with the conditioning state and the service environment. We will tell you whether the tolerance is achievable in unfilled PA, or whether the part needs a glass-filled grade.

Talk to a nylon moulding engineer

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
ko_KRKO

빠른 견적 요청하기

다음을 통해 도면 및 세부 요구 사항을 보내주세요.

Emial: [email protected]

또는 아래 문의 양식을 작성하세요: