LSR Parts With Soft and Hard Patches: Tracing a Metering-Pump Ratio Drift

Ev / Blog

Real moulded silicone seals and O-rings made by Uplastech
Real silicone rubber production context. Uplastech product photo.

The problem

Symptom. An LSR moulding run starts producing parts with soft, tacky streaks beside hard, brittle patches, although the compound lot, mould temperature and cure time are all unchanged.

What it costs. The whole run is scrapped or sorted by hand, and because the fault looks like a bad compound the supplier is blamed while the metering pump keeps drifting into the next batch.

This guide links local hardness to A:B ratio drift, gives a ten-shot weighing test and a hardness map, and sets a ratio and spread limit on the process sheet.

What soft and hard patches mean in a platinum-cured LSR

Two-part LSR is metered at 1:1, with platinum catalyst in A and Si-H crosslinker in B. A pump that slips 5 % changes crosslink density, so one area of a 40 Shore A part cures soft and tacky while another turns hard and brittle.

Finding on the moulded part Most likely cause Confirming check
Soft tacky streak at the flow end B-side shortfall from pump lag Weigh A and B over ten shots
Hard brittle patch near the gate Excess B / crosslinker-rich feed Compare the ratio log for that shift
Same streak on every shot Blocked static mixer channelling Section the mixer and inspect elements
Drift growing through the run Piston seal wear or drum warming Plot shot weight and drum temperature

Table 1 - Reading local soft and hard patches in LSR parts

Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.

Need a fixed price for this seal?

Send the gland drawing, temperature range, media and annual volume. We will recommend a compound with test data and return samples with a written production quotation.

Get a silicone seal quotationEmail [email protected]WhatsApp

Weigh the pump output before blaming the compound

Weigh A and B separately over ten shots on a 0.1 g balance and map hardness at five points per part. The chart below plots Shore A against B-side deviation: a 10 % shortfall drops the flow end to 25 while the gate reads 30.

A five-step diagnostic sequence

  1. Freeze a reference part and the shot log.
    Seal first-article mouldings and record the ratio settings before anyone adjusts the pump.
  2. Weigh A and B over ten consecutive shots.
    Collect each side separately on a 0.1 g balance and compute the ratio for every shot.
  3. Map hardness at five points per part.
    Measure gate, mid cavity and flow end on ten parts, 24 h after moulding, on one durometer.
  4. Inspect the static mixer and pump seals.
    Section the mixer for blocked elements and check piston seal wear against the shot count.
  5. Re-set the ratio and re-map.
    Balance pressures within 2 bar, fit a fresh mixer, and confirm a spread within 3 Shore A.

The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

LSR Parts With Soft and Hard Patches: Tracing a Metering-Pump Ratio Drift: calculated response trend and an illustrative root-cause split
Figure 1 — Calculated response trend and an illustrative root-cause split. Values are engineering guidance for diagnosis, not a measured survey; confirm them on your own line before changing a drawing or a specification.

Set a ratio and hardness-spread limit on the process sheet

Write the ratio check into the process sheet: 1:1 by volume within +/- 2 %, pump pressures balanced within 2 bar, and a 12-element static mixer. Specify 40 +/- 5 Shore A with a 3-point maximum spread per part, measured 24 h after moulding.

Parametre Typical target What goes wrong outside it
A:B metering ratio 1:1 by volume +/- 2 % A 10 % B shortfall drops hardness to 25 Shore A
A/B pump pressure balance Within 2 bar An imbalance lets one side lag each shot
Hardness spread across one part Within 3 Shore A points A wider spread shows local soft and hard zones
Moving-die t90 at 120 C 90 +/- 15 s Past 180 s the B-starved areas stay tacky

Table 2 - Metering and cure parameters to specify for LSR

Separate metering drift from static-mixer channelling

Separate pump drift from mixer channelling: a worn piston seal makes B lag on every shot, while a blocked mixer leaves a fixed streak on one side. A 10 % B shortfall also stretches t90 at 120 C from 90 s past 180 s.

Option When it fits Trade-off
Re-balance A and B pump pressures Ratio drift under 5 % Needs a short line stop
Fit a fresh 12-element static mixer A fixed streak, not a drifting one Consumable cost per run
Replace worn piston seals Drift grows with shot count Pump service and re-qualification
Condition both drums at 23 C Viscosity shifting A-side flow Drum storage and handling space

Table 3 - Corrective options for a drifting LSR metering ratio

Myth: "A process adjustment will fix it." Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.

Hold pump condition and drum temperature through the run

Hold both drums at 23 C so viscosity cannot shift A-side flow, log pump pressure each shift, and replace piston seals every 500,000 shots. Send the mapped part and shot log; we will confirm whether metering or mixing is at fault.

Want a compound check before you re-order?

Send us the gland drawing and the service conditions. We will compare the compound data against your temperature range and return a recommendation with sample parts.

What to send us

  • Gland dimensions and cross-section
  • Temperature range and media
  • A failed seal if available
  • Annual volume

Send the gland drawing

Recovery actions ranked by press downtime

Recover the run by re-weighing ten shots, re-balancing pump pressures within 2 bar, and fitting a fresh mixer, then re-mapping five points on ten parts. If the spread still exceeds 3 Shore A, stop and service the pump rather than raising mould temperature.

Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.

Before you release this silicone seal

  • A 1:1 by volume ratio within +/- 2 % is written into the process sheet
  • A and B pump pressures balanced within 2 bar are recorded each shift
  • A 12-element static mixer and its change interval are specified
  • Hardness is mapped at five points with a 3-point maximum spread
  • Shot weight and drum temperature are logged so drift can be traced

Most cold or heat failures are specification gaps, not bad batches. Fix the specification before changing suppliers.

Why are some areas soft and others hard on one part?

The A:B ratio sets crosslink density. Where B is short the rubber is under-cured and soft; where B is rich it is over-crosslinked and hard. A drifting pump creates both zones in the same shot.

Is a 2 % ratio drift acceptable?

Within +/- 2 % the hardness stays inside 38-42 Shore A and the spread is under 2 points. Beyond 5 % the patches become visible and t90 at 120 C starts to climb; a 10 % shortfall pushes it past 180 s.

How do we tell pump drift from a blocked mixer?

Pump drift changes the ratio over the run and the soft zone moves; a blocked mixer leaves a fixed streak at the same place on every shot. Weigh ten shots, then section the mixer.

Will a hotter mould fix the tacky areas?

No. Extra heat may firm the bulk but cannot restore the missing crosslinker. A B-starved area stays tacky because the chemistry is short of Si-H, not short of temperature.

Why does the drift get worse late in a run?

Worn piston seals let the B side lag more with each shot, and drums warming above 23 C thin the A side. Both show up as a rising ratio error in the shot-weight log.

What hardness spread should we accept?

A maximum of 3 Shore A points across one part, measured at five points 24 h after moulding. A wider spread is the clearest sign that metering or mixing is wrong.

Get a seal specified for the real service conditions

Send us the gland drawing and the service conditions. We will recommend a compound with documented test data, review the squeeze, and supply samples with a production quotation.

To get an accurate quote, send:

  • Gland drawing or seal cross-section
  • Temperature range and media
  • Pressure and movement
  • Annual volume and target unit price

Request samples and a quotation

Prefer to talk it through first?

E-posta [email protected] or message us on WhatsApp +86 177 1752 9949. Send a drawing, a sample or a specification and an engineer will reply.

Why buyers work with Uplastech

ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
tr_TRTR

Hızlı Teklif İsteyin

Çizimleri ve ayrıntılı gereksinimleri şu yolla gönderin

Emial: [email protected]

Veya Aşağıdaki İletişim Formunu Doldurun: