Liquid silicone rubber injection moulding, HCR compression moulding, silicone extrusion and sheeting — platinum-cured, 20 to 90 Shore A, in general-purpose, food-contact and medical grades.

Silicone Rubber Product Types

Translucent liquid silicone rubber molded lens and white LSR sealing diaphragm

Liquid Silicone Rubber (LSR) Molding

Two-component platinum-cured LSR injected into a heated steel tool. The fastest route to high-volume precision silicone: tight tolerances, negligible flash, and fully automated demoulding.

Solid silicone rubber compression molded gaskets, pads and grommets in white, grey and red

Solid Silicone (HCR) Compression Molding

High-consistency rubber for thick sections, large parts and low-to-medium volume. Compression and transfer moulding handle geometries that LSR cannot fill economically.

Coiled white silicone rubber extrusion profiles and a black silicone sealing strip

Silicone Extrusion Profiles

Continuous silicone profiles, sealing strips and cord in any constant cross-section. Platinum-cured for odour-free, non-tarnishing seals; cut to length or supplied in coils.

Coils of clear and white platinum-cured silicone tubing in several diameters

Silicone Tubing

Clear, translucent and coloured silicone tubing for fluid transfer, peristaltic pumps and insulation. Medical and food-contact grades available with full documentation.

Assortment of silicone O-rings and die-cut silicone gaskets in white, translucent and black

Silicone Gaskets & Seals

Moulded O-rings, die-cut gaskets and custom sealing profiles. Compression set and durometer selected against your temperature and media, not against a catalogue page.

Black silicone rubber keypad with raised buttons and a sectioned button showing the carbon pill

Silicone Keypads & Buttons

Moulded keypads with conductive carbon pills, tactile webs and backlit legends. Consistent actuation force, tested per key rather than per batch.

Medical grade silicone mask cushion, seal and clear silicone tubing on a clinical surface

Medical Grade Silicone Parts

Mask cushions, seals, septa and fluid paths in grades supported by USP Class VI and ISO 10993 documentation. Made under a controlled, traceable process.

Rolled and flat silicone rubber sheets in white and translucent, cut edges showing thickness

Silicone Sheets & Sheeting

Solid and sponge silicone sheet from 0.5 to 10 mm, in standard sheets or rolls. Slit, die-cut or laminated with adhesive backing to your drawing.

Silicone is not the right answer for every seal — it has poor resistance to petroleum oils and low tear strength compared with PU. Tell us the media and temperature and we will say so if another elastomer fits better.

What Is Silicone Rubber?

Silicone rubber is a synthetic elastomer built on a silicon-oxygen backbone rather than a carbon chain. That backbone is why it behaves unlike any organic rubber: it stays flexible from −60 °C to +200 °C, resists UV and ozone without additives, and does not support combustion into toxic smoke the way halogenated materials do.

For buyers, the practical consequence is a material that tolerates sterilisation, weathering and food contact in the same part — at a price roughly three to five times that of EPDM or nitrile. Specifying silicone where EPDM would do is one of the most common cost mistakes in sealing design.

LSR vs HCR vs RTV — Which Process?

Фактор LSR injection molding HCR compression molding RTV / cast
Вязкость Pumpable, two-component Dough-like, uncured sheet Pourable liquid
Tooling cost $$$ (steel, heated) $$ (steel, heated press) $ (room-temperature mould)
Время цикла 30 s – 3 min 3 – 20 min 4 – 24 h cure
Economic volume 10,000+ 200 – 20,000 1 – 500
Tolerance Best Хорошо Loosest
Лучшее для Small precision parts, high volume Thick sections, large parts, low volume Prototypes, potting, low-volume seals

Process selection. Volume and part thickness decide the route; tolerance usually follows.

Основные свойства

Недвижимость Typical range Practical meaning
Service temperature −60 °C to +200 °C (+250 °C short term) Survives autoclave cycles and under-hood heat
Hardness 20 – 90 Shore A At 20 A the compound is soft and gel-like; at 90 A it behaves almost like a flexible plastic
Elongation at break 100 – 700% High elongation grades suit diaphragms and seals
Tear strength 10 – 50 kN/m Weaker than PU or natural rubber — avoid sharp edges in dynamic seals
Compression set 10 – 30% (22 h at 175 °C) The number that predicts whether a seal still seals after a year
Dielectric strength 20 – 30 kV/mm Used for insulation and cable jacketing
Chemical resistance Good: water, alcohol, dilute acids. Poor: petroleum oils, concentrated acids, ketones Check the media before specifying — this is where silicone projects fail

Indicative values for general-purpose platinum-cured silicone. Grade selection shifts every row.

Silicone Grades

Grade Compliance / feature Typical use
General purpose Standard platinum cure Industrial seals, gaskets, profiles
Food contact FDA 21 CFR 177.2600, LFGB Baking moulds, utensils, beverage tubing
Медицина USP Class VI, ISO 10993 documentation Mask cushions, septa, fluid paths
High temperature Stable to 250–300 °C short term Oven seals, heat shielding
Flame retardant UL 94 V-0 capable grades Transit, electrical enclosures
Conductive Carbon-loaded, 10²–10⁵ Ω·cm Keypad pills, EMI gaskets
Low compression set < 15% at 175 °C Long-life static seals
Oil-bleed / self-lubricating Controlled surface oil Connectors, pierceable septa

Grade families. Certification documents are supplied per project against the specific compound used.

How LSR Injection Molding Works

  1. Two-component metering. Part A and part B are pumped in a 1:1 ratio, mixed and injected within minutes — the addition cure begins as soon as they meet, so the mixing head is the process bottleneck.
  2. Cold-runner or open injection. A cold runner keeps the compound below cure temperature until it reaches the heated cavity; open injection drops a shot directly into the tool.
  3. Heated cavity cure. A steel tool held at 150–200 °C cures the part in 30 seconds to 3 minutes, depending on wall thickness.
  4. Demoulding. LSR's low surface energy means parts release cleanly — often picked by robot, which is why LSR suits high-volume automation.
  5. Post-cure (optional). A 2–4 hour bake removes volatiles for medical and food-contact parts, reducing outgassing in service.

Dimensional Tolerances

Dimension Class M1 Class M2 Class M3
Up to 4 mm ±0.08 mm ±0.10 mm ±0.15 mm
4 – 16 mm ±0.15 mm ±0.20 mm ±0.25 mm
16 – 40 mm ±0.25 mm ±0.35 mm ±0.40 mm
40 – 100 mm ±0.45 mm ±0.50 mm ±0.70 mm

Simplified from ISO 3302-1 tolerance classes for moulded rubber products. Confirm the class on the drawing — it changes part price more than any other single line.

Flash is the specification nobody writes down. On rubber parts, the acceptable flash line, its location, and whether it may be trimmed by hand or must be deflashed cryogenically will decide both the tool design and your unit price. Agree it at RFQ stage, with a limit sample — not after the first shipment.

Приложения

  • Medical and laboratory — mask cushions, septa, peristaltic tubing, instrument seals.
  • Food and beverage — baking moulds, dispensing tubing, dairy seals, ice-cube trays.
  • Automotive and transit — weatherseals, connector seals, vibration isolators, cable grommets.
  • Электроника — keypads, thermal interface pads, potting and encapsulation.
  • Промышленность — oven and autoclave seals, diaphragm valves, high-temperature gaskets.
  • Consumer — wearable bands, baby products, kitchenware, collapsible containers.

Контроль качества

Incoming compound is checked for durometer, specific gravity and cure state before it reaches a press. In process, we monitor cavity pressure and cure time; on the finished part we test durometer, dimensions, compression set and, where specified, tensile and tear properties. For medical and food-contact work, the compound certificate and post-cure record travel with the batch.

Tell us the media, temperature and hardness — we will specify the compound

Send a drawing or a sample with your annual volume. We will recommend LSR, HCR or extrusion, quote the tooling, and flag it if another elastomer would serve you better and cost less.

Request a quote

Frequently Asked Questions

What is the difference between LSR and solid silicone?

LSR (liquid silicone rubber) is a two-component pumpable compound injected into a heated tool — fast cycles, tight tolerances, high volume. Solid silicone (HCR) is a dough-like compound compression or transfer moulded — slower, cheaper tooling, better for thick sections and lower volumes.

What hardness can you mould?

From 20 to 90 Shore A. At the soft end the compound is difficult to demould and dimensionally less stable; at 90 A it behaves more like a flexible plastic than a rubber, and a TPE or TPU may be the better choice for that application.

Is silicone rubber food safe?

Food-contact grades are available that meet FDA 21 CFR 177.2600 and LFGB requirements. The grade matters, not the material family — always specify the compliance you need, and we will supply the compound certificate with the batch.

Can silicone be bonded to plastic or metal?

Yes, with primer systems or by mechanical interlocking, and it can be overmoulded onto engineering plastics in a two-shot process. Adhesion should be validated on your actual substrate before tooling is committed.

What is the minimum order quantity?

The minimum order is 1,000 pieces for moulded silicone parts. Extruded profiles are quoted by length rather than by piece, usually from 300–1,000 metres, because they run continuously rather than in cycles.

How long does tooling take?

LSR tools typically run 25–40 days including sampling; compression moulds 15–25 days. Add 3–7 days for first-article approval, and expect one correction loop on parts with thin walls or tight flatness requirements.

ru_RURU

Запросите быструю цитату

Отправьте чертежи и подробные требования по электронной почте

Emial: [email protected]

Или заполните контактную форму ниже: