PBT and PET Injection Molding: Glass Fibre, Drying and Warpage

Glass-filled PBT injection moulded electrical connector bodies with metal contacts on an inspection tray
Glass-filled PBT connector bodies with contacts inserted. Thin walls, tight pin positions, V-0 flame rating and a 260 °C solder excursion — this is the application PBT was designed for.

Why PBT owns electrical connectors

Polybutylene terephthalate is a semi-crystalline polyester that does one job better than anything else in its price bracket: it holds thin walls, tight dimensions and a flame rating through a soldering process. Almost every connector body, bobbins, relay base, sensor housing and terminal block in a modern appliance is glass-filled PBT.

PET is the same chemistry with a different chain length and crystallisation behaviour. It is cheaper and tougher in some grades, but it crystallises slowly, which makes it harder to mould and mostly confines it to extrusion, blow moulding and bottles — though glass-filled PET is used for automotive and electrical parts where its higher melting point is worth the difficulty.

The number that governs PBT: glass-fibre loading of 15 – 30 %, which brings shrinkage down from 1.7 – 2.3 % to 0.3 – 0.8 % and raises HDT from 60 °C to 200 °C+. Unfilled PBT is almost never used for structural parts; the filler is what makes the material useful, and it is also what causes the warpage.

Grades

Grade Key property Used for
Unfilled PBT Tough, good surface, low HDT Cosmetic parts, low-temperature
PBT + 15 % GF Balance of flow and stiffness Thin-wall connectors
PBT + 30 % GF Modulus 9 – 10 GPa, HDT 205 °C Structural electrical parts
PBT + 30 % GF, V-0 UL94 V-0 at 0.8 mm Connectors, bobbins, chargers
PBT + GF, hydrolysis resistant Retains strength after 1,000 h at 85 °C / 85 % RH Automotive under-bonnet, appliances
PBT + GF, low warp (mineral/glass) Isotropic shrinkage Flat parts, long thin parts
PBT + GF, impact modified Notched Izod 90 – 130 J/m Parts with snap fits or latches
PBT/ASA, PBT/PC blends Improved surface, lower warp Automotive exterior trim
PET + 30 % GF HDT 220 °C, higher melting point Under-bonnet, higher temperature
PET + GF, nucleation added Faster crystallisation Makes PET mouldable at reasonable cycle times

Table 1 — PBT and PET grade families. The flame-retardant and hydrolysis-resistant variants are the two that matter most in electrical work.

Drying: the same trap as PC, one step milder

PBT and PET are polyesters, and polyesters hydrolyse. Water at melt temperature cleaves the ester bond, reducing molecular weight. The limits are less severe than polycarbonate's but the mechanism is identical.

Материал Maximum moisture Drying If too wet
PBT unfilled 0.04 % 120 °C, 3 – 4 h Silver streaks, brittleness
PBT + 30 % GF 0.04 % 120 °C, 3 – 4 h Streaks, weak weld lines
PBT FR 0.04 % 120 °C, 4 h Streaks plus reduced flame performance
PET + 30 % GF 0.02 % 130 °C, 4 – 6 h Severe hydrolysis — molecular weight collapses
PET unfilled 0.02 % 130 °C, 4 – 6 h Not normally injection moulded

Table 2 — Drying limits. PET is twice as sensitive as PBT and needs a hotter dryer.

The practical point: PBT arrives in sealed foil bags with a moisture barrier, and it should stay there until it goes into the dryer. A bag left open overnight in a humid plant will pick up 0.1 – 0.2 %, which is four times the limit. If the plant has no desiccant dryer and relies on a hot-air oven, the resin will stabilise around 0.05 – 0.08 % on a humid day and the parts will streak.

Myth: "the streaks are just cosmetic — the part is fine." With polyesters they are not cosmetic. The streaks are the visible evidence that the molecular weight has dropped. A streaked PBT connector will pass a dimensional check and fail a pin-retention or a drop test. Purge and re-dry; do not sort and ship.

Processing window

Параметр PBT PET + GF
Температура расплава 240 – 265 °C 275 – 295 °C
Barrel profile 230 / 245 / 255 / 255 °C 260 / 275 / 285 / 290 °C
Mould temperature 60 – 90 °C 100 – 130 °C
Injection pressure 80 – 130 MPa 90 – 140 MPa
Injection speed Быстрый Быстрый
Hold pressure 50 – 70 % of injection 50 – 70 %
Residence time < 6 min < 5 min
Shrinkage, unfilled 1.7 – 2.3 % 1.5 – 2.0 %
Shrinkage, 30 % GF 0.3 – 0.8 % 0.2 – 0.6 %
Regrind Up to 20 % Up to 15 %

Table 3 — Processing windows. The PET mould temperature of 100 – 130 °C is what forces it to crystallise.

The PET mould temperature is not a preference. PET crystallises slowly, and below about 90 °C it cools into an amorphous state that is brittle, dimensionally unstable and will deform if it later sees heat — a phenomenon that shows up as parts warping in a reflow oven. A PET tool needs hot-oil mould temperature control, not water. That single requirement is why PBT dominates and PET is a specialist choice.

Warpage: the main PBT problem

Glass-filled PBT warps because the fibres align with the flow. Shrinkage in the flow direction is 0.2 – 0.4 %; across the flow it is 0.6 – 1.0 %. That difference is the warpage driver, and it gets worse as the flow length increases and the walls get thinner.

Lever Effect Стоимость
Равномерная толщина стенок Large reduction Design change only
Symmetric gating (centre gate, or two gates) Large reduction Tool change
Higher mould temperature Moderate reduction Longer cycle
Lower glass loading (30 % → 15 %) Moderate reduction Lower stiffness — may need thicker walls
Mineral/glass hybrid filler Large reduction Slightly lower strength
Longer fill time Small reduction Время цикла
Post-mould fixture cooling Complete, but adds a process Fixture plus labour

Table 4 — Warpage levers for glass-filled PBT, in order of effectiveness.

For a flat part, the most effective single change is usually the gate: a centre gate makes the flow radial, so the fibre orientation is symmetric about the centre and the part stays flat. An edge gate makes the flow unidirectional, the fibres align along the part, and it curls.

Electrical and flame-retardant grades

Requirement What to specify Watch out for
UL94 V-0 at 0.8 mm FR grade with a halogenated or halogen-free system Halogen-free FR grades often need higher melt temperature
Comparative tracking index > 600 V Specific CTI grade Standard FR grades are 250 – 400 V
Glow-wire, 960 °C GWIT/GWFI rated grade Required for appliance connectors in Europe
Reflow solder resistance PBT with high HDT, or PPA/PA6T PBT can blister at 260 °C if moisture is present
Hot-wire ignition FR grade plus wall thickness Thin walls lose V-0 rating — check the thickness on the certificate
Hydrolysis resistance Hydrolysis-stabilised grade Standard PBT fails after 500 – 1,000 h at 85/85

Table 5 — Electrical requirements. The wall-thickness caveat on V-0 is the one that catches designers.

That last caveat deserves detail: a V-0 rating is always quoted at a specific thickness. A grade rated V-0 at 1.5 mm is often only V-2 at 0.8 mm. If your design has a 0.6 mm wall in a flame-rated part, the certificate you were given does not apply to it. Always check the thickness column on the UL yellow card, not just the rating.

Design rules

Характеристика Rule Why PBT is different
Wall thickness 0.8 – 3.0 mm; thin walls are a strength PBT fills thin sections well; that is why it is used for connectors
Wall uniformity Within 20 % Warpage is the main risk
Ribs 0.5 × wall Thick ribs warp the face
Bosses Wall 0.6 × nominal
Draft 0.5 – 1° PBT releases reasonably well
Gate Centre or symmetric; avoid long unidirectional flow Fibre orientation drives warpage
Pin positions Allow ±0.05 mm on moulded holes; drill if tighter Glass-filled PBT holds holes well but not to machining tolerance
Snap fits Strain ≤ 1.5 % for glass-filled Glass reduces elongation at break to 2 – 3 %
Sharp corners Internal R ≥ 0.5 × wall Glass-filled materials are notch sensitive
Metal inserts Design for 0.5 % differential expansion PBT expands 30 – 60 × 10⁻⁶/K

Table 6 — PBT design rules. Glass-filled grades have low elongation, so snap fits need care.

Inserts and assembly

Most PBT parts are assembled with metal contacts, and the insert design determines whether the part survives.

Метод Suitability for PBT Примечания
Moulded-in inserts Good, with pre-heating Pre-heat to 100 – 120 °C; cool the pin if the wall is thin
Ultrasonic insertion Превосходно The standard method for connectors
Heat staking Хорошо Works well on glass-filled PBT
Press fit Ярмарка Glass-filled PBT is brittle; hoop stress can crack the boss
Self-tapping screws Good in unfilled; poor in 30 % GF Glass causes the boss to split
Ultrasonic welding Хорошо Needs a proper joint design; glass content reduces weld strength
Laser welding Хорошо Requires a transmissive and an absorptive grade
Adhesive Ярмарка Surface energy is moderate; some structural acrylics work

Table 7 — Assembly methods. Self-tapping screws in 30 % GF PBT are a common field failure.

Defects and causes

Дефект Причина Fix
Silver streaks Moisture above 0.04 % Dry at 120 °C for 4 h; check dew point
Brittle parts Hydrolysis, or excess regrind Check moisture and regrind ratio; verify the grade
Деформация Fibre orientation, asymmetric cooling Symmetric gating; uniform walls; higher mould temperature
Short shots on thin walls Cold mould, low speed Raise mould temperature and injection speed
Weld line weakness Low mould temperature, glass accumulation at the weld Raise mould to 80 – 90 °C; move the gate so the weld is not in a loaded area
Flash Low viscosity, high melt temperature Lower melt; check clamp tonnage
Blisters after soldering Absorbed moisture flashing at reflow Dry before moulding; store parts dry; consider a bake before reflow
Ejector pin marks / white stress marks Over-packing, insufficient draft Reduce hold; add draft; increase ejector area

Table 8 — PBT defects. The blister row is a moisture problem that appears a process step later.

Thin-wall filling: what PBT can and cannot do

PBT's reputation comes from its ability to fill thin sections at high speed, which is what connectors need. The limit is a combination of wall thickness, flow length and glass loading.

Wall thickness Flow length, unfilled Flow length, 30 % GF Minimum practical
0.4 mm 25 – 35 mm 15 – 25 mm Specialist tooling only
0.6 mm 45 – 60 mm 30 – 45 mm Achievable with a hot runner
0.8 mm 70 – 95 mm 50 – 70 mm Standard connector practice
1.0 mm 100 – 130 mm 70 – 100 mm Comfortable
1.5 mm 170 – 220 mm 120 – 160 mm Comfortable
2.0 mm 240 – 310 mm 170 – 230 mm Easy

Table 9 — Flow length for PBT at 255 °C melt and 80 °C mould. Glass-filled grades are roughly 30 % shorter.

Below 0.6 mm the process becomes unforgiving: the melt front freezes before the cavity fills, and every variable — mould temperature uniformity, injection speed, gate size — has to be right. That is achievable in a connector tool built for it, and it is not achievable in a general-purpose tool being pushed past its design.

Hydrolysis: the slow failure

PBT and PET degrade in hot humid environments through hydrolysis of the ester bond. This is different from the moisture problem at the hopper — it happens in service, over months, and it is invisible until the part fails.

Condition Standard PBT Hydrolysis-stabilised PBT
85 °C / 85 % RH, 500 h 60 – 75 % strength retention 90 – 95 %
85 °C / 85 % RH, 1,000 h 35 – 50 % 80 – 90 %
85 °C / 85 % RH, 2,000 h 15 – 30 % 70 – 80 %
Hot water immersion, 90 °C Fails within 500 h 2,000 h+
Steam autoclave Not suitable Not suitable

Table 10 — Hydrolysis resistance. The stabilised grade is roughly 3× the service life in hot humid conditions.

The applications that need it are obvious once you know: washing-machine components, dishwasher parts, automotive under-bonnet, anything in a bathroom, anything in a tropical climate. The applications that get caught out are the ones where nobody thought about humidity — a connector in an unheated warehouse in Southeast Asia, or a sensor housing on a pump.

The test that reveals it: 1,000 hours at 85 °C / 85 % RH, then a tensile test. A standard PBT loses half its strength; a stabilised grade loses 10 – 20 %. If a part is going to spend its life above 60 °C and 60 % RH, run that test on the candidate grade before the tool is cut.

PBT, PPS or PA for a connector

Requirement PBT + 30 % GF PA66 + 30 % GF PPS + 40 % GF
Continuous temperature 120 – 140 °C 100 – 120 °C 200 – 220 °C
Dimensional stability in humidity Превосходно Бедный Превосходно
Pin position tolerance ±0.05 mm ±0.15 mm (grows) ±0.05 mm
V-0 without additives Нет Нет Да
Impact strength Низкий Высокий Низкий
Relative material cost 1× 1.1× 3 – 4×
Tooling cost 1× 1× 1.3 – 1.6×

Table 11 — Connector material selection. PBT wins on cost plus stability; PPS wins on temperature; nylon wins on impact only.

The pin-position row is the deciding one for most connectors. A PA66 connector grows 0.3 – 0.6 % after moulding as it absorbs moisture, which on a 40 mm connector body is 0.12 – 0.24 mm of pin movement. That is more than the insertion tolerance of most terminals. PBT does not move, which is why it is the default.

Frequently asked questions

PBT or nylon for a connector?

PBT, almost always. Nylon absorbs moisture and grows, which moves the pin positions; PBT does not. PBT also holds a V-0 rating more easily and is stiffer at the same glass loading. Nylon wins only where impact strength matters more than dimensional stability.

Why is PET harder to mould than PBT?

Because PET crystallises slowly. It needs a mould at 100 – 130 °C with hot-oil control, and even then the cycle is longer. Unfilled PET cooled below 90 °C comes out amorphous and will deform if it later sees heat. PBT crystallises fast enough to run on a water-heated tool.

Can I use 50 % glass-filled PBT?

It exists and it is used for very stiff parts, but the elongation at break drops to about 1.5 % and the material becomes quite brittle. It also wears the tool aggressively. Above 30 – 35 % glass, check whether the design can be met with ribs instead.

How do I stop glass-filled PBT warping?

Gate from the centre so the fibre orientation is symmetric, keep the wall uniform, and run the mould hot (80 – 90 °C). If the part is still out, switch to a mineral/glass hybrid grade, which shrinks more isotropically at the cost of some strength.

Does PBT need annealing?

Not usually. It is sometimes annealed at 120 – 140 °C for 1 – 2 hours to relieve stress in parts that will be machined or that must hold tolerance through a soldering process.

What is the difference between V-0 at 0.8 mm and V-0 at 1.5 mm?

They are different ratings for the same grade. A material rated V-0 at 1.5 mm may only be V-2 at 0.8 mm. If your part has a 0.8 mm wall, the 1.5 mm rating does not apply and the part is not compliant. Always read the thickness column on the UL yellow card.

Can PBT survive lead-free reflow?

Standard PBT is marginal at 260 °C. Grades with higher HDT, or PPA and PA6T, are the usual answer for reflow-compatible parts. If PBT is used, the part must be dry — moisture flashing at reflow temperature causes blisters that look like material failure.

Why do my PBT parts crack around self-tapping screws?

Because 30 % glass-filled PBT has about 2 % elongation at break. The hoop stress from the screw exceeds it. Use an ultrasonic insert, a heat-staked insert, or a larger boss with a thread-forming screw designed for brittle plastics.

Designing a connector or bobbin in PBT?

Send the drawing, the flame rating you need and the soldering process. We will tell you the right glass loading, whether the wall thickness meets the UL rating, and where the tool needs to gate to stay flat.

Talk to a PBT moulding engineer

Последние сообщения

WhatsApp
Facebook
Twitter
LinkedIn
Pinterest
Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
ru_RURU

Запросите быструю цитату

Отправьте чертежи и подробные требования по электронной почте

Emial: [email protected]

Или заполните контактную форму ниже: