Clamping Force and Tonnage Selection: The Five-Step Calculation

Chart of cavity pressure by material and clamping force against projected area for injection molding
Clamping force is the one machine number that decides whether a tool runs clean or flashes, and it is arithmetic, not experience.

Why tonnage is the first number to get right

Every injection moulding quotation starts with a machine size, and that size is set by clamping force. Get it too low and the tool flashes at the far corner of the parting line, no process setting fixes it, and the moulder spends a week blaming the tool. Get it too high and the mould vents are crushed shut, parts burn, and the tool wears out years early.

The number is not a matter of judgement. It is projected area multiplied by cavity pressure, with a small safety margin. The difficulty is that cavity pressure is not the same as injection pressure, and the projected area is not the same as the part footprint.

Two mistakes cause most tonnage errors. Using hydraulic pressure instead of cavity pressure — they differ by a factor of five to ten. And forgetting the runner: on a multi-cavity tool the runner's projected area can add 30–50% to the total.

The arithmetic

Clamping force has to exceed the separating force that the melt exerts on the mould faces. That force is cavity pressure times the projected area of everything the pressure acts on.

F (kN) = A (cm²) × P (bar) ÷ 100

Where A is the total projected area — parts plus runner plus overflow — and P is the peak cavity pressure during packing, not during fill. Then multiply by a safety factor of 1.1 to 1.2.

단계 What to measure Common error
1. Projected area Outline of the part as seen from the nozzle, in cm² Using the flat base area, not the maximum outline
2. Number of cavities Multiply per cavity Forgetting the runner and sprue
3. Cavity pressure Peak pack pressure, from a sensor or a material table Using hydraulic or injection pressure instead
4. Separating force A × P ÷ 100 Mixing units — mm² with bar gives nonsense
5. Safety factor × 1.1 – 1.2 Using 2.0 and oversizing the machine

Table 1 — The five steps of a tonnage calculation. Steps 1 and 3 are where the errors live; the arithmetic itself is trivial.

A worked example. A flat ABS housing, 180 × 120 mm outline, one cavity, a runner with 40 cm² of projected area. Total projected area is 216 + 40 = 256 cm². ABS packs at around 500 bar. Separating force is 256 × 500 ÷ 100 = 1,280 kN, or 128 tonnes. With a 15% margin, the machine needs 150 tonnes.

Cavity pressure by material

Cavity pressure is a material property as much as a process setting. Viscous, fast-freezing, glass-filled or semi-crystalline resins need more pressure to fill and pack the same geometry.

재료 Typical cavity pressure Note
PE, PP 200 – 400 bar Low viscosity, easy flow
PS, HIPS 300 – 500 bar Fast freezing, short flow
ABS 400 – 600 bar Common baseline for tonnage tables
PC 500 – 800 bar High viscosity, needs hot mould
PA6 / PA66 600 – 1,000 bar Crystalline, fast setting
POM 800 – 1,200 bar Very high, narrow process window
PC/ABS 500 – 800 bar Blend, between the two parents
Glass-filled (30%) Add 30 – 50% Viscosity rises with filler loading
Thin wall (under 1 mm) Add 50 – 100% Flow length to thickness ratio dominates

Table 2 — Cavity pressure ranges. These are pack pressures, not fill pressures; a thin-walled part can need double the table value.

The table values assume a reasonably balanced wall thickness and a flow length to thickness ratio under about 150. A part with a 0.8 mm wall running 120 mm from the gate has a ratio of 150 and sits at the limit; a 0.6 mm wall over the same distance needs pressures well outside the range and is usually a tooling problem rather than a tonnage problem.

Projected area: what actually counts

Projected area is the shadow the mould cavity casts on the parting plane. It is not the surface area of the part, and it is not the area of the part's largest flat face.

기능 Counts toward projected area? 왜
Part outline at the parting line 예 This is what the pressure pushes apart
Runner and sprue 예 They carry the same pressure
Side actions, sliders Only the projected face Sliders have their own force balance
Deep ribs, bosses No extra Inside the outline
Undercuts formed by lifters No extra Within the outline
Overflow wells 예 They fill with melt at pressure
Hot runner manifold 아니요 It is behind the stationary platen, not between the halves

Table 3 — What belongs in the projected area. The runner is the item most often left out, and on small parts it is often larger than the part itself.

On a 16-cavity tool making a 3 cm² part, the parts contribute 48 cm² and the runner can contribute 30 cm² or more. Ignoring the runner understates the tonnage by 40%, which is exactly the margin that separates a clean part from a flashed one.

What too little clamping force looks like

Flash is the obvious symptom, but it is the last one to appear. The earlier signs are more diagnostic.

Symptom What it tells you
Flash at the furthest point from the sprue Parting faces are deflecting, not opening evenly
Part weight varies shot to shot Melt is escaping, so pack is inconsistent
Flash appears only at high pack pressure Tonnage is marginal — it is a pressure limit, not a tonnage limit
Flash on one side only Platen parallelism or mould face wear, not tonnage
Short shots that come and go Operator is raising pack pressure to compensate, which makes flash worse

Table 4 — Reading the symptoms. Flash on one side only is a parallelism problem and adding tonnage will not fix it.

The trap is that raising pack pressure to fix a short shot increases the separating force, so a marginal tool starts flashing. The operator backs off the pressure, the short shot returns, and the job runs in a narrow band between two defects. That is the signature of a machine that is one size too small.

What too much clamping force costs

Oversizing is the more common error because it feels safe. It is not free.

Effect Mechanism
Crushed vents Vent depth is 0.02–0.05 mm; tonnage closes it
Burns and dieseling at the end of fill Air cannot escape, so it compresses and ignites
Higher energy consumption Tonnage is a direct power draw
Mould wear and fretting on the parting line Repeated elastic deflection of the faces
Difficulty setting up Small adjustments produce large pressure changes
Tie bar strain and platen deflection Especially on older machines without force monitoring

Table 5 — The cost of oversizing. Vent crushing is the one that turns a good tool into a tool that burns parts for the rest of its life.

A mould built for 100 tonnes run on a 250-tonne press will usually work, because most presses can be set to a lower clamp force. The real risk is a moulder who does not set it down, or a press without a clamp force display, where the machine simply closes at full tonnage.

Verifying the number on the machine

The calculation gives a starting point. The machine gives the answer. Three checks confirm it.

First, the flash test: reduce clamp force in 10% steps until flash just appears at the furthest point, then add back 15–20%. That is the true minimum for the tool at that pressure.

Second, the vent check: with the calculated tonnage applied, inspect the vents. If they are bright and polished, they are being crushed. If they hold a faint witness mark, they are working.

Third, the platen check: on a large mould, place pressure-sensitive film or lead wire at the four corners of the parting line and close at production tonnage. Uneven impressions mean the platens are not parallel and the tonnage is not distributed, whatever the display says.

Choosing the machine, not just the tonnage

Tonnage is necessary but not sufficient. Three other numbers decide whether a machine can run a tool.

Machine parameter Rule of thumb What goes wrong
Shot size Part + runner between 25% and 75% of barrel capacity Below 25%: long residence time, degradation
Injection pressure Cavity pressure × 2 at the nozzle, minimum No headroom, process drifts through the shift
Tie bar spacing Mould width plus 50 mm each side Mould will not fit, or fits with no room for hoses
Daylight and stroke Part depth × 2 plus 100 mm Part cannot be ejected
Screw diameter Matches shot size, not tonnage Oversized screw, long residence time

Table 6 — Machine selection beyond tonnage. Shot size below 25% of barrel capacity is the most common hidden problem on small parts run on large presses.

The shot size rule is worth emphasising. A 20 g part on a machine with a 500 g barrel spends twenty-five times as long in the barrel as it should, and the material degrades. The part may pass inspection and still fail in service because the molecular weight has dropped. A smaller barrel on the same tonnage is almost always the better machine.

How do I calculate clamping force?

Projected area in cm² multiplied by peak cavity pressure in bar, divided by 100, gives kilonewtons. Divide by 9.81 for tonnes, then add 10–20% margin. Include the runner and every cavity.

What cavity pressure should I use?

200–400 bar for PE and PP, 400–600 for ABS, 500–800 for PC, 600–1,000 for nylon, up to 1,200 for POM. Add 30–50% for glass-filled grades and up to 100% for walls under 1 mm.

Is tonnage the same as clamping force?

In practice yes — "tonnage" is shorthand for clamping force expressed in metric tonnes. A 150-tonne machine can apply about 1,470 kN of clamp force.

Why does my part flash even though the tonnage is correct?

Usually one of three things: the parting faces are worn or not parallel, the projected area was underestimated because the runner was left out, or the pack pressure is higher than the value used in the calculation. Check parallelism before adding tonnage.

Can I use a bigger machine and just turn the tonnage down?

Yes, if the machine has a working clamp force setting and the shot size still falls in the 25–75% band. On a small part in a large barrel, the residence time problem is worse than any tonnage benefit.

How much safety margin should I add?

10–20%. More than that and you start crushing vents and wasting energy. The margin is there to cover material batch variation and temperature drift, not to cover a wrong projected area.

Does the number of cavities change the tonnage?

Yes, linearly for the parts, and it also adds runner area. An 8-cavity tool needs eight times the part area plus the runner, which is why multi-cavity tools move to larger presses quickly.

What is a safe minimum shot size?

25% of barrel capacity. Below that the melt residence time becomes long enough to degrade heat-sensitive materials, and the process becomes sensitive to any interruption in the cycle.

Not sure which press a tool needs?

Send us the part drawing, the resin and the cavity count. We will come back with the projected area, the cavity pressure, the tonnage and the machine specification — before you commit to a tool.

Talk to an injection molding engineer

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
ko_KRKO

빠른 견적 요청하기

다음을 통해 도면 및 세부 요구 사항을 보내주세요.

Emial: [email protected]

또는 아래 문의 양식을 작성하세요: