Silicone Heat Ageing: What Fails, and How Fast

Racks of black silicone parts being loaded into a laboratory ageing oven by an operator in gloves
Seventy two hours at 225 C is the standard test. Service is years at 150.

What heat actually does to silicone

The siloxane backbone is one of the most thermally stable polymer chains there is, which is why silicone survives temperatures that would destroy any organic rubber. The weakness is not the backbone but everything around it: the crosslinks, the filler treatment, the additives and the residual volatiles.

At moderate temperatures the material continues to crosslink slowly, which makes it harder and less elastic. At higher temperatures the side groups on the chain begin to oxidise, which makes the surface chalky and eventually brittle. Above about 250 C the filler starts to affect the network and the material loses cohesion.

The practical consequence is that a silicone part rarely fails by melting or by suddenly losing strength. It fails by becoming stiff, losing its compression set resistance and then cracking at a stress concentration. The end of life is a mechanical failure caused by a chemical change.

That is why heat ageing is measured by retention of tensile strength and elongation rather than by appearance. A part that looks fine can have lost half its elongation and be unable to survive a bend that it took easily when new.

The retention curve, and the 25 degree rule

The chart on the left shows tensile strength retained against ageing time for the same compound at 200, 225 and 250 C. At 200 C it retains 78 percent after 336 hours and 66 percent after 672. At 250 C it is down to 38 percent at 336 hours and 22 at 672.

The rule of thumb is that the reaction rate doubles for every 10 to 15 C in organic polymers, and for silicone the effective interval is closer to 20 to 25 C. The curves in the chart are consistent with about 25 C: 672 hours at 200 C gives the same retention as roughly 170 hours at 225 C and 50 hours at 250 C.

That rule is what makes a short test useful. Seventy two hours at 225 C is a week of laboratory time and it predicts years of service at 150 C, within a factor of two or three. It is not a precise prediction, and it should not be presented as one, but it ranks compounds reliably.

The 70 percent line on the chart is the conventional limit for a part that has to keep working. A compound that crosses it at 336 hours at 250 C is not suitable for continuous service at 250 C, whatever its data sheet says about maximum temperature.

Tensile strength retained falling with ageing time at 200, 225 and 250 degrees Celsius with a 70 percent limit marked, and a bar chart of failure mechanisms
Left: retention against time at three temperatures. Right: what actually fails.

The five mechanisms

Further crosslinking at 32 percent is the largest single mechanism. It makes the material harder, reduces elongation and raises compression set. On a seal it is the mechanism that ends the life, because a harder seal takes less deflection and seals less well.

Loss of plasticiser and volatiles at 24 percent is the mechanism that shows first. A silicone that contains a plasticiser or a volatile process aid will lose it in the first hours at temperature, and the part shrinks and hardens. A post cured compound has already lost them, which is one reason the post cure matters.

Oxidation at 20 percent affects the surface before the bulk. Oxygen diffuses into the surface layer and attacks the side groups, which produces a chalky film. That film is a barrier, so the reaction slows, but the chalk is also a crack initiation site on a part that flexes.

Filler degradation at 14 percent and hydrolysis at 6 percent complete the list. Filler degradation matters at the top of the temperature range; hydrolysis matters in humid or steam service, where water attacks the filler-matrix bond.

Running the test properly

The standard test is ASTM D573: age the specimens in an air circulating oven at the specified temperature for the specified time, then test them at room temperature after conditioning. The air circulation matters, because a static oven builds up degradation products that change the result.

The oven has to be at temperature before the specimens go in, and the specimens have to be spaced so that air reaches all surfaces. A stack of specimens in a closed container is not a heat ageing test, it is a different experiment.

Test at least three times: the unaged control, the midpoint and the end point. Two points give a line; three give a check on whether the mechanism changed, which it often does. A curve that drops steeply and then flattens indicates a surface mechanism; one that accelerates indicates the network is failing.

Condition Duration Used for Acceptance
200 C 72 h General high temperature 70 % retention
225 C 72 h Automotive under bonnet 70 % retention
250 C 168 h Severe service 50 % retention
200 C 1000 h Service life approximation 50 % retention
Steam, 150 C 168 h Hydrolysis resistance 60 % retention

Table 1 — Common ageing conditions and acceptance limits

Making a compound last longer

The first lever is the base polymer. A methyl vinyl silicone with a high vinyl content crosslinks more densely and resists further crosslinking better. A phenyl silicone extends the upper temperature range by 20 to 30 C at a significant cost.

The second is the post cure. A proper secondary vulcanisation removes the volatiles that would otherwise be lost in service, and it completes the crosslinking so that the material does not continue to harden in the application. It is the cheapest improvement available.

The third is the filler. A well treated fumed silica with a high surface area resists degradation better than a cheap precipitated filler. The difference shows at 250 C after 168 hours, and it does not show at all in a short test at 200 C.

The fourth is heat stabilisers. Iron oxide and cerium oxide are used to scavenge the radicals that drive oxidation, and they extend life at the top of the range. They also change the colour, which is why high temperature grades are often red or brown.

Predicting service life without guessing

The method is straightforward: test at three temperatures, plot the time to a chosen retention limit against the reciprocal of absolute temperature, and extrapolate. If the three points fall on a straight line, the mechanism is the same at all three and the extrapolation is defensible. If they do not, the mechanism has changed and the extrapolation is not valid.

The extrapolation should never go more than about 30 C below the lowest test temperature. Beyond that the uncertainty is larger than the answer, and a life prediction of 20 years is not something a 72 hour test can support.

The practical approach in most specifications is simpler and more honest: state a test condition and a retention limit, and let the part be qualified against it. That does not predict service life, but it does ensure that two suppliers are being compared on the same basis.

Change Gain Costo Where it shows
Proper post cure Plus 20 to 30 C of life Oven time First 100 hours
Higher vinyl base Plus 10 to 15 C Materiale Long term
Phenyl silicone Plus 20 to 30 C Two to four times the cost Above 250 C
Treated fumed silica Plus 10 C Materiale Above 225 C
Iron oxide stabiliser Plus 10 to 15 C Material, colour Above 225 C

Table 2 — What each change buys, and where it shows

The post cure is first because it is a process step that most specifications require anyway. A compound that fails a heat ageing test without a post cure has not been tested; it has been tested incorrectly.

How long does silicone last at 200 C?

A general purpose compound retains about 70 percent of its tensile strength after 300 to 400 hours at 200 C, and about 50 percent after 1000. A high temperature grade lasts two to three times longer. The number depends far more on the compound than on the temperature alone.

What is the 25 degree rule?

The rate of degradation roughly doubles for every 20 to 25 C rise. It is a rule of thumb for ranking and for extrapolating, not a precise prediction, and it only holds while the failure mechanism stays the same.

Why does silicone get harder with age?

Further crosslinking. The network continues to form new bonds at temperature, which stiffens the material, reduces elongation and raises compression set. It is the dominant ageing mechanism for most silicone compounds.

Does a post cure improve heat ageing?

Considerably. It removes the volatiles that would otherwise be lost in service and completes the crosslinking, which typically buys 20 to 30 C of equivalent life. It is the cheapest improvement available.

Why does my part look fine but fail a bend test?

Because heat ageing reduces elongation before it reduces tensile strength, and the change is invisible. A part that has lost half its elongation will crack at a stress concentration without any visible surface change.

Can I predict 20 year life from a 72 hour test?

Not reliably. The extrapolation is only valid within about 30 C of the test temperature, and only if the mechanism is unchanged. Use the test to rank compounds and to qualify against a specification, not to promise a service life.

Silicone part in a hot application?

Send the service temperature, the time at temperature and the part drawing. We will recommend a compound and the ageing test that actually qualifies it.

Ask about heat ageing

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
it_ITIT

Chiedete un preventivo rapido

Inviare disegni e requisiti dettagliati via

Emial: [email protected]

Oppure compilate il modulo di contatto qui sotto: