Fine bubbles that survive a full cure usually entered at the metering and mixing stage and cannot be removed by mould venting alone.

What the failure looks like on the line

Liquid silicone rubber parts are produced at high cavitation, so one under-cured cavity can pass an average-based check and still fail in the field.

Cut sections show scattered spherical voids, and the count rises after a component drum change or a mixer service.

Two-component LSR is pumped, metered and statically mixed under pressure; leaks, drum changes and viscosity mismatch draw air into the stream. Once dispersed as fine bubbles, the gas is too slow to diffuse out during a short cure, so it is frozen into the part.

Start with the failure as it is reported, not with the parameter that is easiest to measure. On a buyer's specification this distinction matters: a part can measure inside tolerance and still fail in use, because the drawing records geometry while the complaint records behaviour. Component vacuum degassing is usually the first value both sides compare, and it is also the one most often quoted without the conditions attached to it.

The process window that decides it

Four variables move this result more than the rest. The ranges below are illustrative engineering guidance for a first discussion; confirm them on your own tool, material grade and part geometry before they become contract terms.

Variabel Typical window What fails outside it
Component vacuum degassing 10-50 mbar for 10-30 min Insufficient vacuum leaves dissolved air in the drum
A:B metering ratio 1:1 within 1% Ratio drift changes viscosity and entrains air
Static mixer elements 12-24 elements Too few elements leave unmixed pockets that hold gas
Injection fill speed 10-60 mm/s Fast filling traps air ahead of the flow front

Table 1. Starting window for a joint process trial. Values are engineering guidance, not a measured survey.

Component vacuum degassing is typically held at 10-50 mbar for 10-30 min. Insufficient vacuum leaves dissolved air in the drum Record it together with the measurement point and the moment in the cycle; a single number without a location is not a process setting.

A:B metering ratio is typically held at 1:1 within 1%. Ratio drift changes viscosity and entrains air When this drifts, the symptom usually appears at one cavity, one sheet position or one lane before it appears across the whole batch.

Static mixer elements is typically held at 12-24 elements. Too few elements leave unmixed pockets that hold gas A change here is cheap during a trial and expensive after tooling release, so treat it as a controlled variable with a documented re-approval.

Injection fill speed is typically held at 10-60 mm/s. Fast filling traps air ahead of the flow front Put it on the change-control list, otherwise an unannounced material or setting substitution will be mistaken for ordinary process noise.

Reading the response curve

LSR Voiding: Air Trapped at Metering, Not Cured Out in the Mould: Void-free castings (%) against Vacuum degassing time (min)
Figure 1. Left: Void-free castings (%) against Vacuum degassing time (min). Right: how audited failures of this type typically split by cause. All plotted values are illustrative engineering guidance, not a measured survey.

The left panel shows void-free castings (%) as vacuum degassing time (min) increases: the response rises from 42 to 98 on the illustrative 0–100 scale. The dashed line at 95 marks a proposed acceptance limit, not a universal standard. Move that line only after the test method and the sample plan have been agreed, otherwise two suppliers can both be compliant and still deliver different parts.

Read the shape rather than a single point. A curve that changes quickly near the limit is more sensitive to ordinary process noise than one that approaches it gradually, and that difference should be reflected in how tightly the setting is controlled and how often it is checked.

Where the causes actually sit

The right panel of Figure 1 splits audited failures of this type into five groups. The percentages are illustrative engineering guidance for prioritising an investigation, not a measured survey and not a prediction for your line.

Karena Illustrative share First check
Air drawn at drum change 30% Inspect drum seals and follower plates for air ingress.
Metering ratio drift 24% Verify the A:B ratio with a shot-weight check before the run.
Inadequate vacuum degassing 20% Pull a vacuum-degassed sample and compare void count against the production part.
Mixer element shortage 14% Count static mixer elements after any service.
Fast fill trapping air 12% Review fill speed at the flow-front end, not only the setpoint.

Table 2. Cause split and the corresponding first check. Shares are indicative and sum to 100.

Air drawn at drum change accounts for roughly 30% of the illustrative split. Inspect drum seals and follower plates for air ingress. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.

Metering ratio drift accounts for roughly 24% of the illustrative split. Verify the A:B ratio with a shot-weight check before the run. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.

Inadequate vacuum degassing accounts for roughly 20% of the illustrative split. Pull a vacuum-degassed sample and compare void count against the production part. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.

Checks before sign-off

In practice the sequence below is cheaper to run than a root-cause debate after a rejected delivery.

  1. Inspect drum seals and follower plates for air ingress.
  2. Verify the A:B ratio with a shot-weight check before the run.
  3. Pull a vacuum-degassed sample and compare void count against the production part.
  4. Count static mixer elements after any service.
  5. Review fill speed at the flow-front end, not only the setpoint.

Keep a retained reference sample beside every result. When a batch is disputed, the comparison that settles it is almost always between the retained part and the current one under the same method, not between either part and a number on a drawing. Record the instrument, the operator, the conditioning time and the position on the part or sheet for each reading.

Writing it into the specification and the evidence pack

Specify a maximum void count per unit volume on a cut reference section and require the degassing and metering settings to be recorded for each lot.

Write the requirement as a behaviour at a stated condition, not as a brand of material or a machine setting. State the test method, the conditioning, the sample plan and the rule for deciding a pass. Where a document is needed, ask the supplier for documentation that covers the actual construction and check its scope against your own market before approval; a document for the base material alone does not describe the finished part you are buying.

At first-article approval, freeze the drawing revision, the material and colour identification, the process window, the tool and cavity identification, and the inspection method. Any later change to grade, site, tool, or window should trigger a new first article rather than a paper waiver. Keep retained samples from the approved lot and from each production lot so that a future comparison is possible.

Evidence item What it must show
Approved drawing and revision The exact geometry and tolerances the decision applies to
Material and colour identification Grade, supplier, colour reference and any declared recycled content
Process window and change log The agreed settings and any deviation since approval
Inspection record and retained samples Method, conditions, results and a physical reference from the same lot

Table 3. Minimum evidence pack for a first-article decision and a later batch dispute.

None of the figures above should be read as a measured survey. They are engineering guidance for framing a joint trial; confirm them on your own tool, grade and geometry before they become contract terms.

Questions buyers ask

Is this a material problem or a process problem?

Two-component LSR is pumped, metered and statically mixed under pressure; leaks, drum changes and viscosity mismatch draw air into the stream. Once dispersed as fine bubbles, the gas is too slow to diffuse out during a short cure, so it is frozen into the part. It is worth separating the two before a supplier changes a grade: hold the material constant for one controlled run, then move one setting at a time. If the symptom follows the setting, the material was never the cause.

Can component vacuum degassing be traded against cycle time?

Only within the window stated in Table 1, and only with a recorded trial. Insufficient vacuum leaves dissolved air in the drum A faster cycle that sits outside the window usually moves the failure downstream, where it costs more to find.

What should be recorded at incoming inspection?

Keep the measurement, the method, the sample identity and the conditions together. Inspect drum seals and follower plates for air ingress. A result without its conditions cannot be compared with a later batch.

Does a change of LSR require re-approval?

Treat any change to material grade, tool, site or process window as a change that needs a new first-article decision. For silicone rubber work the drawing alone is not enough; the process route is part of what was approved.

How many samples are enough for a first-article decision?

There is no universal number. Sample across cavities, lanes, sheet positions or reel lengths so that the spread is visible, not just the average. Agree the sample plan and the acceptance rule with the supplier before the trial starts.

What belongs in the evidence pack?

The approved drawing and revision, the material and colour identification, the process window, the inspection method and results, the retained reference samples, and documentation covering the actual construction. Ask the supplier to state the scope of each document and check it against your own market.

Seeing this on a current silicone rubber job?

Send the drawing, the material and grade, the process window you are running, and the point in the cycle or the shelf life where the fault appears. We will help you separate a material question from a process question and a specification question before anyone changes a tool.

Talk to our silicone rubber team

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
id_IDID

Minta Penawaran Cepat

Kirim gambar dan persyaratan terperinci melalui

Emial: [email protected]

Atau Isi Formulir Kontak di bawah ini: