The surface heats first and cools first
Infrared energy is absorbed in the first few tenths of a millimetre of the sheet. The surface therefore reaches temperature long before the core, and the core is what has to be at forming temperature for the part to form without thinning out or tearing.
In the 3 mm polypropylene sheet in the chart, the surface reaches 152 degrees Celsius after 40 seconds of heating while the core is still at 78. At 60 seconds the surface is 166 and the core 116, a gap of 50 degrees. The gap peaks around 56 degrees before the two converge.
If the operator sets the cycle by watching a pyrometer on the surface, the sheet leaves the oven with a surface at 175 and a core at 170, which happens to work. But if the heater power drops, or the sheet is a different colour, the surface can still read 175 while the core is at 140, and the part will form badly with every instrument reading normal.
This is the single most common reason a process that ran for months suddenly stops working after a heater change or a resin lot change. The surface reading is preserved and the core is not.
Surface and core, measured together
The practical method is to instrument both. A calibrated infrared pyrometer aimed at the sheet gives the surface temperature continuously and non-contact. An embedded thermocouple, or a contact probe used on a sacrificial sheet immediately after the oven, gives the core.
The embedded probe is made by drilling a fine hole into the edge of a sheet, inserting a fine thermocouple, and sealing the entry with the same polymer. The probe then travels with the sheet through the oven and records the core temperature in real time.
Do this once per material and thickness, and you have a curve that tells you the relationship between the surface reading the machine gives you and the core temperature you actually need. After that, the pyrometer is a usable proxy, provided you re-check when anything changes.
The chart on the left is exactly that pair of curves. The value is not the numbers, it is the gap: it tells you that a surface reading of 152 corresponds to a core of 78 at 40 seconds and to a core of 170 at 120 seconds. Without the second curve, the first is ambiguous.

Which instrument, and what it gets wrong
An infrared pyrometer is fast and non-contact, and its accuracy depends entirely on the emissivity setting. Polymer sheet emissivity is typically 0.90 to 0.95, but it falls for thin or glossy sheet and for some colours. A pyrometer left at the factory default of 0.95 will read low on a shiny black sheet and high on a white one.
A contact probe is accurate but slow, and it cools the surface it touches. It is suitable for spot checks on a sacrificial sheet, not for continuous control.
A thermal camera gives a full field and is the best tool for finding distribution problems, which is why it is used for oven mapping. Its absolute accuracy is worse than a pyrometer and its relative accuracy is excellent, so use it to find the pattern and a probe to confirm the level.
Whatever the instrument, calibration matters more than the type. A pyrometer that is two years old and never checked is a source of confident wrong numbers.
| Instrument | Reads | Akurasi | Best use |
|---|---|---|---|
| Infrared pyrometer | Surface, non-contact | Good if emissivity set | Continuous surface |
| Contact probe | Surface, contact | Good but slow | Spot checks |
| Thermal camera | Surface field | Relative excellent | Oven mapping |
| Embedded thermocouple | Core | Luar biasa | Window development |
Table 1 — What each instrument actually measures.
Finding the forming window
The forming window is the range of sheet temperature in which the part forms without defects at both ends. Below it the sheet is too stiff and the part tears or does not draw into corners. Above it the sheet sags, the plug assist marks it, and the wall thins excessively.
The window is not the same width for every material. In the right hand panel, PP spans 150 to 175 degrees, HDPE 125 to 145, PS 120 to 155, PVC 130 to 165 and PET 165 to 195. PET has the widest window and the highest temperature; HDPE has the narrowest and the lowest.
A narrow window means the temperature control has to be tighter, which means the measurement has to be better. Running HDPE on a 20 degree process tolerance is not possible, because the whole window is 20 degrees.
Map the window once per material and thickness by forming a series of parts at increasing temperature and recording where each defect appears. The result is a chart that the setters can use, and it converts a skill into a procedure.
| Bahan | Forming window | Width | Practical tolerance |
|---|---|---|---|
| PP | 150 to 175 C | 25 C | +/- 6 C |
| HDPE | 125 to 145 C | 20 C | +/- 4 C |
| PS | 120 to 155 C | 35 C | +/- 8 C |
| PVC | 130 to 165 C | 35 C | +/- 8 C |
| PET | 165 to 195 C | 30 C | +/- 7 C |
Table 2 — Window width sets how tight the temperature control has to be.
Emissivity, colour and thickness
Emissivity is the ratio of the energy a surface emits to what a black body at the same temperature would emit. For most opaque polymer sheet it sits between 0.90 and 0.95, which is convenient. For thin translucent sheet it can drop below 0.7, and the pyrometer will read a temperature that is too low by tens of degrees.
Colour matters because pigments change both the absorption spectrum and the emission. Black sheet absorbs infrared strongly and heats fast; white sheet reflects much of it and heats slowly. A pyrometer calibrated on natural sheet will be wrong on both.
Thickness matters because a thin sheet reaches the core temperature quickly and the surface-core gap is small, so a surface reading is nearly correct. A thick sheet has a large gap, so a surface reading is nearly useless.
The fix is to calibrate the pyrometer against a contact probe on the actual sheet, at the actual colour and thickness, at forming temperature. It takes twenty minutes and it removes an entire class of unexplained process drift.
A procedure that holds
First, establish the window for each material and thickness by forming parts across a temperature range and recording the defects. Second, establish the surface-to-core relationship with an embedded probe. Third, calibrate the pyrometer on the real sheet.
Then write the setpoints as core temperatures with a surface reading as the proxy, and note the colour and grade the proxy was established on. When any of those change, the proxy has to be re-established.
Finally, keep a reference sheet. A known sheet of the same material, heated on a known cycle and measured at a fixed point, will reveal a heater or reflector problem before it reaches production. It is the cheapest instrument in the plant.
Why does my pyrometer read a temperature that cannot form the part?
Because it reads the surface and the surface is hotter than the core during heating. The core is what has to be at forming temperature, and the gap can reach 50 degrees or more.
How do I measure the core temperature of a sheet?
Drill a fine hole into the sheet edge, insert a fine thermocouple, seal the entry with the same polymer, and run the sheet through the oven. The probe records core temperature in real time.
What emissivity should I set on the pyrometer?
Between 0.90 and 0.95 for opaque sheet, lower for thin translucent sheet. Calibrate against a contact probe on the actual colour and thickness rather than trusting a default.
What is the forming window for PET?
About 165 to 195 degrees Celsius, which is the widest of the common materials but also the highest. PP is 150 to 175 and HDPE only 125 to 145.
Why does the process drift after a heater change?
The surface reading can be preserved while the core is not, so the pyrometer looks normal and the sheet is under-heated. Re-establish the surface-to-core relationship after any heater work.
Is a thermal camera better than a pyrometer?
For finding distribution problems, yes. For absolute temperature, no. Use the camera to find the pattern and a probe to confirm the level.
Parts failing with normal instrument readings?
Send the material, thickness and cycle. We will help you establish the surface-to-core relationship and a forming window you can hold.