Mould Venting: Depth, Position and the 0.02 mm That Prevents a Burn

Close view of a mould face with shallow milled vent grooves running from the cavity edge, a feeler gauge blade slipped into one groove, a magnifier beside
Vent grooves on a parting face, checked with a feeler gauge. Twenty microns is the difference between a full shot and a burnt one.

Air is the last thing to leave

A cavity is full of air before it is full of plastic. The plastic arrives at the gate at a few hundred bar and pushes the air ahead of it, and the air has to leave through the parting line, through a vent, or through the ejector pin clearances. If it cannot leave, it compresses.

Compressed air gets hot. A cavity that fills in half a second and cannot vent will compress the air at the end of the flow to a pressure that raises its temperature several hundred degrees, and the plastic at that point scorches. That is a burn: a black or brown patch, always at the last place to fill, always with a sharp edge on the upstream side.

The confusing part is that a burn looks like a material problem and is a tool problem. The first response is usually to drop the melt temperature or slow the injection, both of which reduce the burn and both of which cost cycle. A vent costs nothing after the tool is cut and nothing to run.

Depth is a window between two failures

A vent has to be shallow enough that the plastic does not enter it and deep enough that the air can. Those two requirements produce two curves that cross, and the crossing is the working depth.

At 0.005 mm of vent depth the burn rate is 24 percent, because the vent is effectively closed. At 0.010 it is 11, at 0.015 it is 4.2, at 0.020 it is 1.1, at 0.025 it is 0.5 and at 0.030 it is 0.3. The burn curve falls steeply and then flattens.

The flash curve does the opposite. At 0.005 mm it is 0.1 percent, at 0.015 it is 0.4, at 0.020 it is 0.9, at 0.025 it is 2.4 and at 0.030 it is 7.8. It rises slowly and then steeply, because once the gap is wide enough for the melt to enter, the entry is fast.

The two curves cross at about 0.021 mm, and that is why the standard vent depth for most commodity plastics is 0.02 mm. It is not a rule of thumb, it is the intersection of two failure modes, and it moves with the material: a low viscosity grade needs a shallower vent, a glass filled one a slightly deeper one because the glass does not flow into a 0.02 mm gap.

Burn rate falling from 24 percent at 0.005 millimetres vent depth to 0.3 at 0.030, and flash rate rising from 0.1 to 7.8, crossing near 0.021 millimetres
Left: burn rate falling and flash rate rising against vent depth, crossing near 0.021 mm. Right: burn rate against vent count on the same total vent area, 6.2 percent with one vent and 0.7 with eight.

Position beats depth

Once the depth is in the window, the next gain comes from where the vents are. On the same total vent area, one vent gives a burn rate of 6.2 percent. Two give 3.1, four give 1.4, six give 0.9 and eight give 0.7.

The reason is that air does not flow sideways along a parting line. It leaves where the flow front pushes it, which is the last point to fill, and if that point has no vent the air has to travel to find one. A long thin cavity with a vent at one end is a cavity with a burn at the other end, no matter how deep the vent is.

Which means the vent layout comes from a fill simulation or from a short shot, not from a habit. The short shot is the cheap version: run the tool at 80 percent fill, look at where the flow front stops, and put a vent there. Repeat at 90 and 95 percent, because the last place to fill moves as the pressure rises.

Burn rate falling from 6.2 percent with one vent to 0.7 percent with eight vents on the same total vent area
Burn rate against vent count at constant total vent area. Distributing the vents is worth more than deepening them.

Where the vents have to go

The end of the flow path is the first place. On a simple part that is the far edge from the gate; on a part with ribs it is the end of each rib, because a rib fills last and its tip is a dead end.

A weld line is the second. Two flow fronts meeting trap the air between them, and a weld line with no vent is a weld line with a burn in it. A vent at the weld line also improves the weld strength, because air in the weld is what makes it weak.

A blind boss or a deep pocket is the third, and it is the one most often missed. A boss fills from the bottom and the air has nowhere to go, so a small vent at the top of the boss is worth more than a large one on the parting line.

The fourth is the gate itself, on the opposite side. Air can be pushed back through the sprue if the machine allows it, but a vent at the far end of the runner is what stops the air being pushed into the cavity in the first place.

The four kinds of vent

A parting line vent is a shallow groove milled into the parting face, running from the cavity edge to the outside of the block. It is the cheapest, it is the easiest to clean, and it is the one that wears: the parting face is what takes the clamp load, and a groove in it closes up over time.

An ejector pin clearance is a vent that already exists. A pin in a hole with 0.02 to 0.03 mm of clearance vents the cavity at no cost, which is why a part with a burn at an ejector pin is a part with a blocked pin.

A porous steel insert is a block of sintered metal set into the cavity wall. Air passes through the metal, the plastic does not, and it vents an area rather than a line. It is used on a deep blind pocket and on a part where a groove is impossible, and it clogs and needs cleaning.

A vacuum system pulls the air out before the shot. It is the most effective and the most expensive, it needs a seal around the cavity and a valve, and it is used where the other three cannot do the job: a very thin wall, a very fast fill, or a part with nowhere to put a groove.

Typ Depth Cleaning Verwenden Sie
Parting line groove 0.02 mm Easy Default
Ejector pin clearance 0.02-0.03 mm With the pin Free, if the pin is there
Porous steel insert Material Difficult Blind pocket, deep boss
Vacuum Not applicable Seal check Thin wall, fast fill

Table 1 — Vent types and where each one is the right answer

Vents clog, and that is the maintenance item

A 0.02 mm groove is 20 microns wide. It fills with plasticiser, with mould release, with a film of the polymer itself, and with the dust that is in every workshop. The burn comes back, slowly, and the first response is usually to raise the injection speed, which makes it worse.

The cleaning is a brass scraper and a solvent, on a schedule rather than on a symptom. A vent that is checked every shift and cleaned when it needs it never produces a burn; a vent that is cleaned when the parts go black produces a burn every few months and a scrapped batch with it.

The measurement is the feeler gauge in the photo. A 0.02 mm blade should pass and a 0.03 mm blade should not. If the 0.02 blade will not pass, the vent is closed; if the 0.03 passes, the vent has worn and the flash is on its way.

Symptom Ursache Fix
Burn at the last point to fill Blocked or missing vent Clean, or add a vent
Flash along the parting line Vent worn too deep Re-cut, or move the vent
Burn at a weld line No vent at the meeting point Add a vent there
Burn at a boss Blind pocket Porous insert or a vent at the top

Table 2 — Reading the symptom back to the vent

Myth: a deeper vent is a safer vent. Depth is a window, not a minimum. Past about 0.025 mm the burn stops improving and the flash starts, and at 0.030 mm the flash rate is seven times what it was at 0.020.

How deep should a mould vent be?

0.02 mm for most commodity plastics, because that is where the burn curve and the flash curve cross. Low viscosity grades want less, glass filled grades a little more.

Why does my part burn at the last place to fill?

Because the air has nowhere to go and it is being compressed. A vent at that point, not a lower melt temperature, is the fix.

Is one big vent as good as several small ones?

No. On the same total area, one vent gives a 6.2 percent burn rate and eight give 0.7 percent, because air leaves where the flow front pushes it.

Can ejector pins vent a mould?

Yes, through their clearance, at 0.02 to 0.03 mm. A burn at an ejector pin usually means the pin or the hole is blocked.

How do I check a vent?

With a feeler gauge. A 0.02 mm blade should pass and a 0.03 mm blade should not; if the 0.02 will not pass the vent is closed.

When is vacuum venting worth it?

On a very thin wall, a very fast fill, or a part with nowhere to put a groove. It is the most effective and the most expensive option.

A part that burns at the end of fill, or flashes at the parting line?

Send the part, the gate position and a short shot. We will tell you where the vents belong and what depth the material needs.

Ask about venting

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
de_DEDE

Fordern Sie ein schnelles Angebot an

Senden Sie Zeichnungen und detaillierte Anforderungen über

Emial: [email protected]

Oder füllen Sie das untenstehende Kontaktformular aus: