The problem

Symptom. A panel that looks flat as moulded shows a clear shadow of every rib after the 120 C paint bake and high-gloss topcoat, so a passing first article becomes a rejected Class-A surface.

What it costs. The fault is found only after painting, the most expensive step, so whole batches are scrapped or reworked while moulder and painter argue over which inspection condition applies.

This guide links the rib-to-wall ratio to measured sink depth before and after coating, and defines a painted-part acceptance limit to agree before tooling.

Why a rib shadow appears only after coating

A rib at 0.8 times the nominal wall leaves a 38 um sink that is invisible as moulded, yet a 120 C paint bake and high-gloss topcoat roughly double it to a legible shadow on the finished panel.

Observed symptom Most likely cause First check on the line
Faint rib line only after painting Sink telegraphing through the coating Profile unpainted and painted panels from one shot
Shadow matches every rib exactly Rib-to-wall ratio too high Measure rib and wall thickness on section
Depth grows after the bake Stress release at 120 C Measure before and after the paint oven
Only one rib reads through Local cooling or a long unsupported rib Log the rib position against the cooling layout

Table 1 - Reading the shadow before re-cutting the rib

Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.

Need a fixed price for this moulded part?

Send the 2D drawing, resin grade and annual volume. Our engineers return a DFM review, a material recommendation and a written quotation you can compare line by line.

Get a moulding quotationEmail [email protected]واتساب

Measure sink on unpainted and painted panels

Profile the sink across the rib with a profilometer on unpainted and painted panels from one shot. A jump from 12 to 26 um at a 0.6 ratio is telegraphing, not a new dent.

A five-step diagnostic sequence

  1. Profile the rib on unpainted and painted panels from one shot.
    A doubling of depth after coating confirms telegraphing rather than handling damage.
  2. Section the part and measure rib against wall.
    A ratio above 0.6 on a 2.5 mm wall is the design root cause.
  3. Record hold pressure, mould temperature and cooling.
    A 45 MPa pack at 90 C leaves more root shrink than 60 MPa at 70 C.
  4. Compare against the 20 um legibility limit.
    Define the gloss and viewing distance so a borderline panel is measurable.
  5. Thin the rib in the tool, then re-paint and re-measure.
    Process tuning buys margin; only a thinner rib removes the cause.

The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

Rib Sink Telegraphing Through Paint: Why a Flat Panel Shows Its Bones: calculated response trend and an illustrative root-cause split
Figure 1 — Calculated response trend and an illustrative root-cause split. Values are engineering guidance for diagnosis, not a measured survey; confirm them on your own line before changing a drawing or a specification.

Rib-to-wall ratio and root radius for the drawing

Keep ribs at 0.5-0.6 times a 2.5 mm wall, so 1.3-1.5 mm, with a root radius under 0.25 mm, to hold sink below the 20 um legibility limit on the drawing.

المعلمة Typical target What goes wrong outside it
Rib to nominal wall ratio 0.5-0.6 At 0.8 the sink exceeds 38 um as moulded
Root fillet radius At most 0.25 mm or 0.25 x wall A large radius adds mass at the rib root
Sink depth after paint bake At most 20 um Above this it reads under a high-gloss topcoat
Hold pressure 50-65 MPa Low pack lets the rib root shrink away

Table 2 - Rib and sink parameters for the drawing

Process settings that move the margin

Higher hold pressure near 60 MPa and a cooler 70 C mould reduce the as-moulded sink, but they cannot rescue a rib that is simply too thick for the wall.

Decision Effect on sink Trade-off
Thin rib from 0.8 to 0.6 x wall 38 um down to about 12 um as moulded Tool change; slightly less stiffness
Raise hold pressure 45 to 60 MPa Reduces root shrink Risk of sticking and higher ejection force
Lower mould temperature 90 to 70 C Skins over sooner Can raise residual stress and post-bake bow
Accept only on painted first articles Tests the real condition Adds a paint step to sampling

Table 3 - Decisions that set painted-panel read-through

Myth: "A process adjustment will fix it." Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.

Define acceptance on the finished part

Agree acceptance on the finished part: a maximum sink depth measured after the full paint bake under a defined gloss and viewing distance, not on the raw moulding.

Not sure whether the fault is in the tool or the process?

Send us the drawing, the process window and a few sample parts. We will tell you which change fixes the fault before you commit to a tool modification.

What to send us

  • Part drawing with the affected dimension
  • Current process settings
  • Sample parts from a good and a bad batch
  • Annual volume

Send the part for review

Sampling rules that catch telegraphing early

Trim hold pressure and extend cooling first; thinning the rib in the steel is the permanent fix. Always re-measure painted panels, because unpainted readings understate the fault.

Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.

Before you release this injection moulding job

  • Rib thickness is specified as a ratio of nominal wall on the drawing
  • Root fillet radius is dimensioned, not left to the toolmaker
  • Maximum sink depth is defined on the painted part after the production bake
  • Gloss level and viewing distance for the visual check are agreed
  • First-article approval includes painted panels from every cavity

Attach this list to the RFQ. Most moulding faults are decided at the drawing stage.

Why is the sink invisible before painting?

A 10-20 um depression scatters little light on a moulded texture. A high-gloss topcoat levels optically and a 120 C bake releases stress, so the same depression reads as a rib shadow.

Is this the same as a normal sink mark?

The mechanism is the same local shrink at a thick rib root, but the dispute here is a part that passed raw inspection and failed after coating, so the acceptance condition must be the painted part.

What rib-to-wall ratio should we use?

0.5-0.6 of the nominal wall is a safe default; on a 2.5 mm wall that means a 1.3-1.5 mm rib with a root radius under 0.25 mm.

Can more hold pressure hide it?

Raising pack from 45 to 60 MPa reduces root shrink, but an oversized rib will still telegraph. Use pressure for margin, not as the fix.

Does a lower mould temperature help?

A cooler 70 C mould skins the surface sooner and can reduce the as-moulded sink, but it may add residual stress that reappears after the paint bake.

Who owns the rejected painted panels?

Define it up front. If the drawing only specifies raw-part flatness, the moulder passes and the painter inherits the claim; specify post-paint sink depth instead.

Get a mouldable part and a fixed quotation

Send us the part file and the failure history. Our engineers will return a DFM review, a material recommendation and a fixed quotation with a defined first-article acceptance test.

To get an accurate quote, send:

  • 3D file or 2D part drawing
  • Resin grade and any regrind limit
  • Annual volume and target unit price
  • The failed sample or defect photos

Request a DFM review and quote

Prefer to talk it through first?

البريد الإلكتروني [email protected] or message us on WhatsApp +86 177 1752 9949. Send a drawing, a sample or a specification and an engineer will reply.

Why buyers work with Uplastech

ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.

أحدث المنشورات

واتساب
فيسبوك
تويتر
لينكد إن
بينتيريست
Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
arAR

اطلب عرض أسعار سريع

إرسال الرسومات والمتطلبات التفصيلية عبر

Emial: [email protected]

أو املأ نموذج الاتصال أدناه: