Post-Cure Residues: Record the 200 C for 4 h Cycle

Real moulded silicone seals and O-rings made by Uplastech
Real silicone rubber production context. Uplastech product photo.

The problem

Symptom. A buyer rejects 4,200 silicone stoppers after headspace GC reads 1,400 ppm total volatiles against a 500 ppm clause, and the oven chart shows the 200 C for 4 h post-cure was skipped.

What it costs. With no post-cure condition or volatile limit in the specification, a batch with odour and fogging complaints is quarantined and the re-work lands on the moulder.

This article links peroxide decomposition by-products to a missing post-cure, gives the 200 C for 4 h condition to be confirmed per formulation, TGA and headspace GC verification, and the clause that binds the oven record.

When an odour complaint meets a skipped post-cure

A buyer rejects 4,200 silicone stoppers after headspace GC reads 1,400 ppm total volatiles against a 500 ppm clause, and the oven chart shows the 200 C for 4 h post-cure was skipped. The parts are dimensionally correct; the residues are not.

What the buyer sees Document behind it First clause to check
Headspace GC reads 1,400 ppm Post-cure omitted 500 ppm total-volatiles clause
Only 'post-cured' on the note No oven chart Dated 200 C for 4 h record
TGA shows high mass loss Volatile residues remain TGA plus headspace GC-MS
Compound changed after the trial Condition no longer valid Re-confirm 200 C for 4 h per grade

Table 1 - Reading a post-cure volatiles gap before booking the lot

Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.

Need a fixed price for this seal?

Send the gland drawing, temperature range, media and annual volume. We will recommend a compound with test data and return samples with a written production quotation.

Get a silicone seal quotationEmail [email protected]WhatsApp

Ask for the oven chart and a volatiles report

Request the post-cure oven chart with time and temperature plus a TGA or headspace GC volatiles report for the lot. Treat the root-cause split as illustrative engineering guidance to confirm on your own line; a 'post-cured' note has no oven record.

A five-step diagnostic sequence

  1. Pull the oven chart.
    Confirm the post-cure reached 200 C for 4 h and that the chart belongs to the shipped lot.
  2. Measure total volatiles.
    Run headspace GC on the lot and compare the 1,400 ppm figure with the 500 ppm clause.
  3. Check by TGA as well.
    Thermogravimetric mass loss shows whether volatile residues remain after cure.
  4. Compare with an uncured control.
    A drop after post-cure confirms the cycle, rather than the compound, is at fault.
  5. Bind the condition in the order.
    Name 200 C for 4 h, the 500 ppm limit and a dated oven chart per lot.

The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

Post-Cure Residues: Record the 200 C for 4 h Cycle: calculated response trend and an illustrative root-cause split
Figure 1 — Calculated response trend and an illustrative root-cause split. Values are engineering guidance for diagnosis, not a measured survey; confirm them on your own line before changing a drawing or a specification.

Peroxide by-products and the 200 C for 4 h condition

Peroxide vulcanisation leaves aromatic ketone and acid by-products that a post-cure drives off at elevated temperature. A typical condition is 200 C for 4 h, but the time and temperature must be confirmed for each compound and section thickness.

Clause or parameter Required value What goes wrong outside it
Cure system Peroxide, named on the order Platinum grade quoted against a peroxide condition
Post-cure condition 200 C for 4 h, confirmed per compound A skipped cycle leaves 1,400 ppm volatiles
Total volatiles Below 500 ppm by headspace GC Odour and fogging complaints
Verification TGA and headspace GC-MS per lot No comparable figure between lots

Table 2 - Post-cure clauses for the part specification and purchase order

TGA and headspace GC verification

Verify by thermogravimetric analysis for total mass loss and headspace GC-MS for individual species, against an uncured control. The 500 ppm clause is an agreed acceptance figure, so state the method, sampling and units that produced it.

Action What it fixes Cost or trade-off
Obtain the oven chart for the lot Closes the record gap Low: a records check
Re-run headspace GC on retained parts Confirms the 1,400 ppm figure Low to medium: laboratory test
Apply the post-cure and re-test Removes the residues Medium: oven cycle and re-test
Re-qualify a low-volatile grade Clears a persistent exceedance High: new compound and re-run

Table 3 - Recovery actions ranked by cost

Myth: "A process adjustment will fix it." Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.

Write the post-cure and volatile limit into the order

On the order name the peroxide cure system, a post-cure of 200 C for 4 h as the starting condition, and a 500 ppm total-volatiles limit by headspace GC. Require a dated oven chart and volatiles report per lot.

Want a compound check before you re-order?

Send us the gland drawing and the service conditions. We will compare the compound data against your temperature range and return a recommendation with sample parts.

What to send us

  • Gland dimensions and cross-section
  • Temperature range and media
  • A failed seal if available
  • Annual volume

Send the gland drawing

Recovery actions ranked by cost

For a held lot, first apply the specified post-cure and re-run headspace GC; re-working an existing batch is the cheapest fix. If volatiles still exceed 500 ppm, move to a platinum-cured low-volatile grade and re-qualify, the costliest route.

Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.

Before you release this silicone seal

  • The purchase order names the cure system and a post-cure of 200 C for 4 h, confirmed for the specific compound
  • A total-volatiles limit of 500 ppm by headspace GC is stated with method, sampling and units
  • A dated oven chart with time and temperature is required per production lot
  • TGA and headspace GC-MS verification is agreed as the evidence method
  • Any compound or section-thickness change triggers a re-confirmation of the post-cure condition

Most cold or heat failures are specification gaps, not bad batches. Fix the specification before changing suppliers.

Why were the stoppers rejected?

Headspace GC read 1,400 ppm total volatiles against a 500 ppm clause, and the oven chart showed the 200 C for 4 h post-cure was skipped.

What does post-cure remove?

Peroxide decomposition by-products, mainly aromatic ketones and acids, that cause odour, fogging and elevated extractables if left in the rubber.

Is 200 C for 4 h universal?

No. It is a typical starting condition that must be confirmed for each compound and section thickness, then written into the order.

Which tests verify it?

Thermogravimetric analysis for total mass loss and headspace GC-MS for the individual volatile species, against an uncured control.

Can a platinum-cured grade skip post-cure?

It has no peroxide by-products, but a low-volatile grade may still be post-cured. Confirm the condition for the chosen compound.

Who owns a skipped cycle?

Put it in the order: name 200 C for 4 h, a 500 ppm limit and a dated oven chart per lot, settled by records.

Get a seal specified for the real service conditions

Send us the gland drawing and the service conditions. We will recommend a compound with documented test data, review the squeeze, and supply samples with a production quotation.

To get an accurate quote, send:

  • Gland drawing or seal cross-section
  • Temperature range and media
  • Pressure and movement
  • Annual volume and target unit price

Request samples and a quotation

Prefer to talk it through first?

Email [email protected] or message us on WhatsApp +86 177 1752 9949. Send a drawing, a sample or a specification and an engineer will reply.

Why buyers work with Uplastech

ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
en_USEN

Ask For A Quick Quote

Send drawings and detailed requirements via

Emial: [email protected]