PPS and PEEK Injection Molding: Hot Moulds and Crystallinity

Amber PEEK and black PPS injection moulded components on a high-temperature test bench beside a thermocouple readout
Amber PEEK and black glass-filled PPS parts. Both were moulded with a tool at 180 °C and a melt above 340 °C — which is why the machine, the oil heater and the tool steel all had to be specified together.

When the material costs more than the machine time

PPS (polyphenylene sulfide) and PEEK (polyether ether ketone) sit at the top of the engineering thermoplastics ladder. PPS holds its properties to 200 °C continuously and is inherently flame retardant. PEEK goes to 250 °C, has outstanding chemical resistance, and is one of the few polymers acceptable for repeated autoclave sterilisation and for direct contact with aggressive solvents.

The economics are unlike any other material in this series. PEEK costs €70 – €120 per kilogram; PPS €12 – €25. A 20 g part in PEEK therefore carries €1.40 – €2.40 of material before any processing. At that ratio, the machine time and the tooling are almost irrelevant — what matters is yield. A 5 % scrap rate on a PEEK part can cost more than the moulding.

The number that governs both materials: mould temperature. PPS needs 130 – 150 °C; PEEK needs 170 – 200 °C. That is above the capability of water-based temperature control, so the tool must be designed for hot oil from the start — conformal cooling channels sized for oil flow, no water lines, high-temperature seals, and a manifold that can take 200 °C. A tool designed for water cannot be converted.

PPS versus PEEK

Proprietà PPS + 40 % GF PEEK + 30 % GF
Continuous use temperature 200 – 220 °C 250 °C
Melting point 280 – 285 °C 340 – 343 °C
Glass transition ~90 °C ~143 °C
Tensile strength, MPa 150 – 190 180 – 220
Flexural modulus, GPa 11 – 14 10 – 13
HDT at 1.82 MPa > 260 °C > 315 °C
Flame rating UL94 V-0 inherently, at 0.4 mm UL94 V-0 at 1.5 mm
Chemical resistance Excellent; no known solvent below 200 °C Excellent; attacked by concentrated sulphuric acid only
Water absorption 0.02 – 0.05 % 0.1 – 0.5 %
Shrinkage, % 0.2 – 0.5 0.3 – 1.4 (grade dependent)
Temperatura di fusione 310 – 340 °C 360 – 400 °C
Mould temperature 130 – 150 °C 170 – 200 °C
Relative material cost 1× 5 – 8×

Table 1 — PPS and PEEK side by side. The cost difference is the reason PPS is used wherever it is good enough.

The decision rule is straightforward: use PPS unless you need above 220 °C, autoclave sterilisation, or resistance to a specific aggressive chemical. PPS is inherently V-0 without additives, which is a significant advantage — flame-retardant PEEK grades exist but are more expensive and less robust. Most "we need PEEK" requirements turn out to be met by PPS at a fifth of the cost.

Grades

Grade family Materiale Key property Used for
PPS + 40 % GF PPS Stiffest, most dimensionally stable Connectors, pump housings, under-bonnet
PPS + 40 % GF + mineral PPS Low warp, good surface Flat parts, automotive
PPS unfilled PPS Tough, low warpage Coatings, chemical parts
PPS impact modified PPS Notched Izod 60 – 90 J/m Parts with snap fits
PEEK unfilled SETTIMANA Maximum toughness and elongation Seals, wear parts, medical
PEEK + 30 % GF SETTIMANA Stiffness plus high temperature Structural, aerospace
PEEK + 30 % CF SETTIMANA Highest stiffness, conductive Bearings, aircraft parts
PEEK, bearing grade PEEK + PTFE + graphite µ 0.10 – 0.20 Bearings, thrust washers
PEEK, medical SETTIMANA ISO 10993, implantable variants Instruments, implants
PEI, PAI, PPSU Adjacent families Between PPS and PEEK Where PEEK is over-specified

Table 2 — High-temperature grade families. PEI (Ultem) and PPSU are worth evaluating before jumping to PEEK.

The machine and the tool

PPS and PEEK cannot be run on a standard machine without modification. The requirements are specific and they are not negotiable.

Item Requirement Reason
Barrel temperature capability 400 – 420 °C for PEEK Standard barrels are rated 350 – 380 °C
Barrel and screw material Bimetallic or corrosion-resistant PPS releases corrosive volatiles at temperature
Screw design Low-compression, wear resistant Glass-filled material is highly abrasive
Nozzle Heated, with a positive shut-off Drool at 380 °C is a real problem
Hot runner Rated 400 °C, with external heating Standard hot runners are rated 300 – 350 °C
Mould temperature control Hot oil, 200 °C capability Water cannot reach 180 °C
Tool steel Hardened, 50 – 54 HRC Abrasion plus high temperature
Tool insulation Insulating plates between tool and platens Otherwise the press acts as a heat sink
Seals and hoses High-temperature rated Standard hoses fail at 180 °C oil
Venting 0.01 – 0.02 mm, generous Trapped gas at 380 °C burns the part

Table 3 — Machine and tool requirements. Any one of these missing stops the job.

The most common planning error is the mould temperature control. A tool quoted with "hot oil capability" but drilled with 8 mm channels sized for water flow will not deliver 180 °C uniformly — the oil flow rate is too low, the pressure drop too high, and the tool runs 30 °C cooler at the far end. Conformal cooling or generously sized channels (12 – 14 mm) are needed, and the oil unit must be sized for the tool's heat load, not just its temperature.

Processing windows

Parametro PPS + GF PEEK + GF
Temperatura di fusione 310 – 340 °C 360 – 400 °C
Barrel profile 290 / 310 / 325 / 330 °C 340 / 365 / 380 / 390 °C
Mould temperature 130 – 150 °C 170 – 200 °C
Injection pressure 90 – 140 MPa 100 – 160 MPa
Injection speed Veloce Moderate — high shear degrades PEEK
Hold pressure 50 – 70 % of injection 50 – 70 %
Residence time < 6 min < 5 min
Drying 150 °C, 3 h 150 – 160 °C, 3 – 4 h
Ricottura Rarely needed 200 °C for 2 – 4 h for maximum crystallinity
Regrind Up to 15 % 0 – 10 % (property loss is significant)

Table 4 — Processing windows. PEEK's 400 °C melt is at the limit of most standard equipment.

Drying is often overlooked because these materials absorb so little water — 0.02 % for PPS. But at 380 °C even 0.05 % moisture causes visible splay and a measurable loss of molecular weight, and the part cost means the scrap is expensive. Dry at 150 °C for 3 hours regardless of what the datasheet implies.

Crystallinity: the property you control with the tool

Both materials are semi-crystalline, and the degree of crystallinity determines strength, wear resistance, chemical resistance and dimensional stability. It is set by the mould temperature and the cooling rate, and it cannot be recovered afterwards except by annealing.

Mould temperature Crystallinity Result
PEEK at 120 °C 15 – 20 % Brittle, poor wear, poor chemical resistance, dimensionally unstable
PEEK at 160 °C 25 – 30 % Acceptable for non-critical parts
PEEK at 180 – 200 °C 30 – 35 % Full properties as specified
PPS at 100 °C Basso Brittle; fails impact
PPS at 140 – 150 °C Alto Full properties

Table 5 — Crystallinity versus mould temperature. A cold tool produces a part that looks right and is not.

This is the single most important thing to understand about high-temperature materials: a PEEK part moulded at 120 °C looks identical to one moulded at 190 °C, passes a dimensional check, and has roughly half the wear life and a fraction of the chemical resistance. If a supplier cannot tell you their mould temperature, they cannot tell you what they made.

Design rules

Caratteristica Rule Perché
Wall thickness 1.5 – 4.0 mm Thin walls are hard to fill at high viscosity; thick walls are expensive material
Wall uniformity Within 15 % Differential crystallinity causes warpage
Internal radius ≥ 0.5 × wall Notch sensitivity in glass-filled grades
Draft 1 – 1.5° High shrinkage force, especially PEEK
Gate Large; direct or edge High shear degrades the melt
Snap fits Strain ≤ 1 % for glass-filled Elongation at break is 2 – 3 %
Threads Avoid; use inserts or a separate fastener Thread roots crack in brittle grades
Material minimisation Core out every non-functional volume At €70 – €120/kg, geometry is the biggest cost lever
Tolerance ±0.05 mm achievable on small parts, ±0.1 mm typical High shrinkage and crystallinity variation limit it

Table 6 — Design rules. The material-minimisation row is unique to this cost bracket.

Cost structure: where the money actually goes

Cost element PPS part PEEK part
Materiale 45 – 60 % 70 – 85 %
Machine time (hot runner, slow cycle) 15 – 25 % 8 – 15 %
Tooling amortisation 10 – 20 % 3 – 8 %
Scrap and yield loss 5 – 10 % 5 – 15 %
Ispezione 3 – 8 % 2 – 5 %

Table 7 — Cost structure. On PEEK, material is the price; on PPS, it is roughly half.

The consequence for design is that a PEEK part should be designed like a machined part: minimise the envelope, core out everything, and accept a more complex tool if it removes material. A 20 % reduction in part volume is a 20 % reduction in the largest cost line, which usually beats any cycle-time improvement.

Where each material belongs

Applicazione Materiale Reason
Automotive under-bonnet connectors PPS + 40 % GF 200 °C, chemical resistance, V-0 inherent
Pump and valve housings PPS + GF Chemical resistance, dimensional stability
LED reflector housings PPS or PEEK High temperature, low outgassing, white grades available
Surgical instruments SETTIMANA Repeated autoclave, ISO 10993
Bearing cages, thrust washers PEEK + PTFE/graphite Wear, temperature, chemical resistance
Aerospace brackets PEEK + CF Specific strength, FST compliance
Semiconductor wet benches PEEK or PPS Resistance to acids and solvents at temperature
Downhole and oilfield parts SETTIMANA Temperature plus H₂S and hydrocarbon resistance

Table 8 — Application map. Most "PEEK" requirements are actually PPS requirements.

Defects and causes

Difetto Causa Fix
Brittle parts Low mould temperature → low crystallinity Raise mould to 140 °C (PPS) or 180 °C (PEEK)
Curvatura Differential crystallinity, fibre orientation Uniform mould temperature; symmetric gating
Splay / streaks Moisture Dry at 150 °C for 3 – 4 h
Black specks Degraded material at 380 °C Purge; check hot-runner dead spots; reduce residence
Short shots Cold tool, high viscosity Raise mould and melt temperature; increase speed
Flash Low melt viscosity at high temperature Check clamp tonnage — high-temperature melts are thin
Vesciche Volatiles, or moisture Dry; add venting; check for degradation
Dimensional drift after machining Incomplete crystallinity Anneal at 200 °C before machining

Table 9 — Defects. Four of the eight trace back to mould temperature or moisture.

Designing a tool for a 200 °C mould

A high-temperature tool is a different design, not the same design with a bigger heater. The differences are structural and they have to be in the tool from the start.

Caratteristica Standard tool High-temperature tool Perché
Cooling channels 8 – 10 mm, water 12 – 14 mm, hot oil Oil needs 3 – 5× the flow for the same heat transfer
Seals Nitrile O-rings Viton or PTFE Nitrile fails at 150 °C
Hoses Standard hydraulic High-temperature rated, insulated Standard hose degrades at 180 °C oil
Insulation None Insulating plates to the platens Otherwise the press is a 20 kW heat sink
Tool steel P20, 30 – 34 HRC H13 or 1.2343, 50 – 54 HRC Abrasion plus thermal cycling
Ejector system Standard Clearanced for thermal expansion A 300 mm steel block grows 0.6 mm at 200 °C
Slides and lifters Standard fits Increased clearance, dry-film lubricant Grease carbonises at 200 °C
Venting 0.02 mm 0.01 – 0.015 mm Thinner melt at temperature flashes more easily
Hot runner 300 – 350 °C rated 400 °C rated, external heat Internal-heat hot runners cannot reach 400 °C

Table 9 — Standard versus high-temperature tooling. The insulation and the thermal expansion allowance are the two most often forgotten.

Thermal expansion deserves a number: steel grows about 12 × 10⁻⁶ per kelvin. A 300 mm mould block taken from 20 °C to 200 °C grows 0.65 mm. If the ejector plate, the guide pins and the slides were fitted at room temperature with standard clearances, the tool will seize at operating temperature. High-temperature tools are assembled with the expansion allowance designed in, and often they are checked hot before the first shot.

Annealing and machining PEEK

PEEK parts are frequently machined after moulding, and the sequence matters. Machining a part with incomplete crystallinity produces a part that changes dimension weeks later.

Passo Condition Scopo
1. Mould Mould at 180 – 200 °C Achieve 30 – 35 % crystallinity in the tool
2. Anneal 200 °C for 2 – 4 h, cool at ≤ 20 °C/h Complete crystallinity, relieve stress
3. Machine Sharp carbide tooling, high speed, low feed PEEK machines like brass but is abrasive when filled
4. Re-anneal (optional) 200 °C for 1 – 2 h Relieve machining stress for tight-tolerance parts
5. Inspect After 24 h at 23 °C Let the part stabilise before final measurement

Table 10 — The PEEK mould-anneal-machine sequence. Skipping step 2 causes dimensional drift after machining.

For implantable or medical PEEK, annealing is also part of the validation: the crystallinity level affects the material's mechanical performance and must be documented. A supplier who cannot state the crystallinity of the parts they ship cannot support a medical submission.

Qualifying a supplier for high-temperature moulding

Domanda Why it matters Acceptable answer
What is your maximum barrel temperature? PEEK needs 400 °C A specific number, not "high"
How do you control mould temperature? Water cannot reach 180 °C Hot oil, with the unit capacity stated
What mould temperature will you run? Determines crystallinity 180 – 200 °C for PEEK, 140 °C for PPS
How do you verify crystallinity? The part can look right and be wrong DSC, density, or a documented process window
What is your dryer dew point? Moisture causes splay and hydrolysis −20 °C or lower, measured
Is the hot runner rated for the melt temperature? Standard units fail above 350 °C A specific rating above the process temperature
What is your regrind policy? Regrind reduces HDT and wear life Stated percentage, and tested
Can you show a DSC trace? It is the only proof of crystallinity Yes, for the actual production parts

Table 11 — Supplier qualification questions. A supplier who cannot answer the crystallinity question should not be quoting PEEK.

The crystallinity question is the one to press on, because it is where a cheap quote comes from. A moulder running PEEK at 140 °C mould temperature will produce parts faster and cheaper, and they will look identical. They will also have roughly half the wear life and a fraction of the chemical resistance — and the failure will appear in the customer's application, not in the incoming inspection.

Frequently asked questions

Do I really need PEEK, or will PPS do?

PPS handles 200 – 220 °C continuously, is inherently V-0, and resists almost every chemical. PEEK is needed above 220 °C, for autoclave sterilisation, for concentrated sulphuric acid, and for the highest wear applications. If none of those apply, PPS at a fifth of the cost is the right answer.

Can I mould PEEK on a standard machine?

Only if the barrel is rated for 400 °C and the tool can run at 180 – 200 °C with hot oil. Most standard machines are rated 350 – 380 °C and most standard tools are drilled for water. Both need to be specified for the material from the start.

Why is my PEEK part brittle?

Almost certainly low crystallinity from a cold mould. PEEK needs 170 – 200 °C to crystallise fully; at 120 °C it is 15 – 20 % crystalline instead of 30 – 35 %. The part looks identical and has roughly half the wear life.

Does PPS need a hot runner?

It benefits from one, but the hot runner must be rated for 400 °C with external heating. A standard 300 °C hot runner will not hold PPS at 330 °C reliably and the tips will freeze or degrade the material.

How much does PEEK tooling cost?

1.3 – 2× an equivalent PBT tool, because of the hardened steel, the hot-oil cooling design and the high-temperature hot runner. The tooling is a small share of the project cost — the material dominates.

Can PEEK be sterilised repeatedly?

Yes — that is one of its defining advantages. PEEK withstands over 1,000 autoclave cycles at 134 °C, plus gamma and ethylene oxide sterilisation, without significant property loss. PPS is not suitable for repeated autoclave.

What is the shrinkage of PEEK?

0.3 – 1.4 % depending on grade and flow direction — a very wide range. Unfilled PEEK is at the high end and is anisotropic; 30 % glass-filled is at the low end. This is why PEEK tools are usually cut, trialled and corrected rather than cut to a calculated shrinkage.

Is regrind acceptable?

Up to 10 – 15 % for PPS, 0 – 10 % for PEEK. The property loss is real and the material is expensive enough that regrind is tempting — but on a part that was specified for high-temperature performance, a 15 % regrind addition can drop the HDT below the requirement. Test it, do not assume.

Specifying a high-temperature part? Check whether PPS is enough before you budget for PEEK

Send the drawing, the continuous service temperature and the chemical environment. We will tell you which material actually meets it, and what the part costs in each.

Talk to a high-temperature moulding engineer

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
it_ITIT

Chiedete un preventivo rapido

Inviare disegni e requisiti dettagliati via

Emial: [email protected]

Oppure compilate il modulo di contatto qui sotto: