The problem
Symptom. An ESD tray that read 2 x 10^7 ohm/sq at first article now measures 3 x 10^11 ohm/sq after 12 weeks, so a whole batch sits outside the dissipative band and no longer protects the boards.
What it costs. Out-of-band trays either let static through or conduct too fast, so electronics are at risk, the lot is rejected at goods-in and the buyer and moulder argue over whether the additive or the test humidity is to blame.
This guide separates migratory additives from permanent compounds, sets the surface-resistance band and 23 C / 50 % RH conditioning, and defines a lot acceptance test.
- 1. What an out-of-band ESD tray looks like
- 2. Separate a migratory additive from a test error
- 3. Resistance and conditioning for the drawing
- 4. Additive, coating and humidity that set resistance
- 5. Define a lot acceptance test for surface resistance
- 6. Recovery actions ranked by requalification cost
What an out-of-band ESD tray looks like
A dissipative tray should sit between 10^6 and 10^9 ohm/sq. A migratory antistat at 2 % loading reads 2 x 10^7 ohm/sq at 23 C / 50 % RH, yet climbs past 3 x 10^11 ohm/sq after 12 weeks in dry stores.
| Observed result | Most likely cause | First check on the order |
|---|---|---|
| Resistance rose to 3 x 10^11 ohm/sq | Migratory antistat dried out | Re-condition 48 h at 23 C / 50 % RH |
| Reading falls after humid conditioning | Humidity-dependent additive | Measure at 100 V per ANSI/ESD S11.11 |
| Tray passes once, fails after a wash | Topical coating wiped off | Repeat the reading after the defined wash |
| Only one corner reads high | Poor additive dispersion | Log resistance by point and by tray |
Table 1 - Reading an ESD tray dispute before rejecting the lot
Need a fixed price for this moulded part?
Send the 2D drawing, resin grade and annual volume. Our engineers return a DFM review, a material recommendation and a written quotation you can compare line by line.
Separate a migratory additive from a test error
Condition 5 trays for 48 h at 23 C / 50 % RH and measure with a concentric ring probe at 100 V. A reading that falls back to 10^7 ohm/sq after humid conditioning is a humidity-dependent additive, not a bad batch.
A five-step diagnostic sequence
- Pull the drawing and the goods-in readings.
Compare the 2 x 10^7 ohm/sq first article with the 3 x 10^11 ohm/sq reading after 12 weeks. - Condition 5 trays for 48 h at 23 C / 50 % RH.
Measure at 100 V with a concentric ring probe to ANSI/ESD S11.11. - Check whether the additive is migratory or permanent.
A 2 % migratory additive dries out; a 15 % carbon-filled PP holds near 3 x 10^6 ohm/sq. - Repeat the reading after the defined wash.
A 0.5 um topical coating that passes once but fails after a wash is not durable. - Re-mould and re-qualify if it stays out of band.
A tray still at 3 x 10^11 ohm/sq needs the permanent compound, not more conditioning.
The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

Resistance and conditioning for the drawing
Put the band on the drawing: 10^6 to 10^9 ohm/sq to ANSI/ESD S11.11 at 100 V, measured after 48 h at 23 C / 50 % RH, with 5 trays per lot and a named permanent antistat compound.
| Parametro | Typical target | What goes wrong outside it |
|---|---|---|
| Surface resistance, ANSI/ESD S11.11 | 10^6 to 10^9 ohm/sq at 100 V | Above 10^11 the tray is insulative |
| Conditioning before measurement | 48 h at 23 C / 50 % RH | Dry trays read four decades higher |
| Antistat type | Permanent compound or 15 % carbon-filled PP | A 0.5 um coating wipes off in service |
| Lot sampling | 5 trays per lot, repeat after wash | A single pass hides a topical coating |
Table 2 - Surface-resistance parameters for the part drawing
Additive, coating and humidity that set resistance
A 0.5 um topical coating wipes off and a 2 % migratory additive needs humidity, rising more than four decades at 12 % RH. A 15 % carbon-filled PP holds near 3 x 10^6 ohm/sq across that range.
| Decision | Effect on resistance | Trade-off |
|---|---|---|
| Switch to 15 % carbon-filled PP | Holds about 3 x 10^6 ohm/sq | Higher resin cost, black colour only |
| Use a permanent antistat compound | Stable across 12 to 50 % RH | Requalify the material and colour |
| Keep the 2 % migratory additive | Cheap at 23 C / 50 % RH | Drifts over four decades in dry stores |
| Re-test only after conditioning | Clears a falsely rejected lot | Does not fix a dried-out additive |
Table 3 - Decisions ranked by requalification cost
Define a lot acceptance test for surface resistance
Agree lot acceptance before first article: 10^6 to 10^9 ohm/sq on 5 trays per lot, 48 h at 23 C / 50 % RH, a 100 V probe, and a repeat reading after the defined wash so a coating cannot pass once.
Not sure whether the fault is in the tool or the process?
Send us the drawing, the process window and a few sample parts. We will tell you which change fixes the fault before you commit to a tool modification.
What to send us
- Part drawing with the affected dimension
- Current process settings
- Sample parts from a good and a bad batch
- Annual volume
Recovery actions ranked by requalification cost
For an out-of-band lot, re-condition at 23 C / 50 % RH and re-measure. A tray that recovers to 10^7 ohm/sq is humidity-dependent; if it stays at 3 x 10^11, re-mould with the permanent compound and re-qualify.
Before you release this injection moulding job
- A surface-resistance band of 10^6 to 10^9 ohm/sq at 100 V is stated on the drawing
- Conditioning of 48 h at 23 C / 50 % RH is written into the test method
- The antistat type is named as a permanent compound or 15 % carbon-filled PP, not a topical coating
- A lot test of 5 trays per lot with a repeat reading after the defined wash is agreed
- First-article approval records resistance by tray and by point to ANSI/ESD S11.11
Attach this list to the RFQ. Most moulding faults are decided at the drawing stage.
Why did resistance rise after 12 weeks?
A 2 % migratory antistat needs moisture. In dry stores it climbed from 2 x 10^7 to 3 x 10^11 ohm/sq, over four decades, leaving the dissipative band.
Is the tray or the test to blame?
Condition 5 trays for 48 h at 23 C / 50 % RH and measure at 100 V. A reading that falls back to 10^7 ohm/sq was a dry tray, not a bad compound.
What band should we specify?
10^6 to 10^9 ohm/sq to ANSI/ESD S11.11 at 100 V, measured after 48 h at 23 C / 50 % RH, with 5 trays per lot.
Additive or coating?
A permanent antistat or 15 % carbon-filled PP holds near 3 x 10^6 ohm/sq across 12 to 50 % RH. A 0.5 um topical coating wipes off and fails after a wash.
Can we just re-condition an out-of-band lot?
Re-conditioning clears a falsely rejected lot, but a dried-out migratory additive drifts again. For a stable tray, specify the permanent compound.
Who owns a rejected ESD lot?
Put it in the order. Name the band, the 48 h at 23 C / 50 % RH conditioning, the 100 V test and the 5-tray lot sample so a reading is judged by one method.
Get a mouldable part and a fixed quotation
Send us the part file and the failure history. Our engineers will return a DFM review, a material recommendation and a fixed quotation with a defined first-article acceptance test.
To get an accurate quote, send:
- 3D file or 2D part drawing
- Resin grade and any regrind limit
- Annual volume and target unit price
- The failed sample or defect photos
Request a DFM review and quote
Prefer to talk it through first?
Email [email protected] or message us on WhatsApp +86 177 1752 9949. Send a drawing, a sample or a specification and an engineer will reply.