Acrylic Rod Sizes, Tolerances and Straightness

Digital vernier caliper measuring the diameter of a transparent acrylic rod
Diameter is the number everyone specifies and the only one many drawings define. Ovality, bow and end finish decide whether the rod actually fits.

1. What sizes are actually available

Acrylic rod is nominally available from about 2 mm to 200 mm, but the range is not uniform across processes, and availability in a given diameter and colour is a stock question rather than a capability question.

Diameter Estruso Cast Note
2–10 mm Standard, 1 mm increments Available, made to order Extruded is the economical route at this size
10–30 mm Standard, 1–2 mm increments Standard, 1–2 mm increments The overlap zone — choose on tolerance and volume, not availability
30–60 mm Available, fewer sizes Standard Extruded tolerance starts to loosen; cooling becomes harder
60–120 mm Not practical Standard, 5–10 mm increments Cast only
120–200 mm+ No Made to order Long cure cycles; expect lead time measured in weeks

"Standard" means commonly held or routinely produced. Non-standard diameters are possible but usually carry a minimum quantity, because a cast mould tube or an extrusion die is dedicated to that size.

Two practical points. First, an odd diameter like 17.5 mm will cost more than 18 mm in almost every case, because it is not a size anyone holds tooling for. Second, if your drawing calls for a nominal that nobody makes, the supplier will either machine it from the next size up — which changes the price entirely — or quietly supply the nearest standard and hope you do not measure.

2. Diameter tolerance: how to write it

This is where most acrylic rod disputes start, because "20 mm" is not a specification and the two processes hold very different tolerances.

Diameter range Extruded — achievable Cast — achievable
2–10 mm ±0.1 mm ±0.3 mm
10–30 mm ±0.2 mm ±0.5 mm, or ±2 %
30–60 mm ±0.3 mm ±1.0 mm, or ±2 %
60–120 mm — ±1.5 mm, or ±2 %
120 mm+ — ±2.0 mm, or ±2 %

Indicative for standard commercial production. Tighter figures are negotiable on extruded rod with in-line gauging; cast rod cannot be brought to extruded tolerance because the mould tube, not a die, sets the size.

How to write it. Give the nominal and a symmetric tolerance — 20.0 ± 0.2 mm — rather than a limit range, unless you specifically need an asymmetric band. State the measurement temperature if the part is large, and state how many points along the length are measured. A tolerance without a sampling rule is not enforceable.

The trap. A drawing that specifies ±0.1 mm on a 40 mm cast rod is asking for something the process cannot do. The supplier has three options: decline, machine the rod down from a larger size (expensive), or accept the order and ship out-of-tolerance. Only the first two are honest, and the second changes the price significantly. If you need that tolerance, say so at the quoting stage.

3. Ovality — the dimension nobody specifies

Ovality is the difference between the largest and smallest diameter measured across the same cross-section, usually expressed as a percentage of nominal. It is almost never on a drawing and it is the reason a rod that "measures 20 mm" will not fit a 20 mm hole.

  • Extruded: typically 1–2 % of diameter. On a 20 mm rod that is 0.2–0.4 mm — the same order as the diameter tolerance itself.
  • Cast: up to about 3 % of diameter, driven by tube roundness and cooling symmetry.

If the rod goes into a close-fitting hole, a bearing, or a collet, specify ovality explicitly. If it is decorative, it does not matter and specifying it only adds cost.

4. Straightness and bow

Straightness is expressed as maximum deviation from a straight line, in millimetres per metre of length. It is a separate requirement from diameter and it is the one most often left out.

Product Typical bow What drives it
Extruded rod, standard 1–2 mm/m Cooling symmetry, haul-off alignment, stress relaxation
Extruded rod, controlled 1 mm/m or better Balanced cooling and a stress-relief pass
Cast rod 2–5 mm/m Tube verticality during cure, cooling symmetry

Two things to state alongside the number. First, the length over which it is measured — a rod that is straight over 500 mm can be visibly bowed over 2 metres. Second, whether the rod is measured as supplied or after conditioning, because a rod packed while still warm can bow in the box.

For long decorative lengths where straightness is a design feature, the practical fix is often not a tighter specification but better packing — a rigid tube or a supported crate rather than a bundle.

5. Length and cut tolerance

Standard supply is 1000 mm or 2000 mm straight lengths; some producers offer 3000 mm in smaller diameters. Cut-to-length is normal and priced per cut.

  • Cut length tolerance: ±1 mm is standard. Tighter needs a different cut-off arrangement and is priced accordingly.
  • Squareness of cut: a saw cut is rarely perfectly square. If the rod has to butt against a surface, specify squareness or specify a machined end.
  • Length and temperature: acrylic expands roughly 0.07 mm per metre per °C. A 2 m rod measured at 30 °C in a warehouse and again at 20 °C in a lab differs by about 1.4 mm — more than the cut tolerance. State the measurement temperature for long lengths.

6. End finish

The end of the rod is usually specified last and matters most, because it is the face people look through.

Finitura What it looks like Use it when
Sawn Matte, with visible saw marks; light scatters Ends are hidden, or will be machined later
Machined square Flat and dimensionally accurate, still slightly matte Ends butt against a surface or are assembled
Polished Clear, transparent through the end face Visible ends, light guides, display parts
Flame polished Very clear, slightly rounded edge Decorative visible ends where a soft edge is acceptable

Polished ends are a separate operation and a separate line item. A quotation that says "cut to length" does not include them, and the difference in cost is not trivial on short lengths.

7. Surface finish and optical grade

Standard rod has a glossy as-produced surface — from the mould tube in casting, from the die and cooling in extrusion. Beyond that there are three grades worth distinguishing.

  • Standard: glossy, minor surface marks acceptable, no optical requirement. Most decorative and structural applications.
  • Optical: specified light transmission (clear PMMA is around 92 % over 3 mm), no visible internal bubbles or haze, ends polished. Light guides, lenses, display components.
  • Protected: standard or optical rod with a peelable film on the cylindrical surface, for parts that must arrive scratch-free and be handled before assembly.

Specifying "optical" without defining a transmission value and a bubble limit gives the supplier nothing to work to. State the transmission, the measurement thickness, and the maximum acceptable defect with a reference sample.

8. Annealed or unannealed

Annealing relieves internal stress. It matters if the rod will be machined, drilled, tapped, cemented or exposed to solvents.

  • Unannealed is normal for rod sold as stock and cut into decorative lengths. Cheaper, and adequate if nothing further happens to it.
  • Annealed is required before machining or solvent cementing. It costs slightly more and prevents the most common field failure in acrylic components — a crack that appears a day after assembly.

Ask for a craze test result rather than a statement that the rod is annealed. It is a short test and it is the only objective evidence.

9. Packing and protection

Acrylic scratches if you look at it wrongly, and packing is where a good rod becomes a rejected rod.

  • Interleaving. Rods packed in direct contact rub in transit. Paper interleaf or individual sleeving prevents it.
  • End protection. Ends take the impact in a dropped carton. End caps or foam are cheap insurance on polished ends.
  • Support. Long lengths need a rigid crate or tube. A bundle strapped in the middle sags and bows.
  • Film. Peelable film on optical grades, applied clean and removed within the stated shelf life — an old film leaves adhesive residue that is worse than the scratches it prevented.

10. A specification you can copy

This is the level of detail that produces a quotation you can compare with another supplier's. Everything below is a decision you have to make anyway; writing it down costs nothing and prevents most disputes.

Parametro What to state Esempio
Materiale PMMA, cast or extruded Cast PMMA, annealed
Colour Reference sample, transparency, diameter for approval Amber, transparent, approved on 20 mm
Diameter Nominal and symmetric tolerance 20.0 ± 0.2 mm
Ovality % of nominal, if it matters ≤ 2 %
Rettilineità mm per metre, and over what length ≤ 2 mm/m over 2 m
Length Length and cut tolerance 1000 ± 1 mm
End finish Sawn, machined or polished Polished both ends
Optical Transmission and defect limit, if applicable ≥ 90 % at 3 mm, no visible bubbles
Stress Annealed, with craze test evidence Annealed, craze test passed
Packing Interleaf, end protection, crate type Paper interleaf, foam ends, rigid crate
Quantity Per order and per year 500 pcs, 2000 pcs/year

11. Frequently asked questions

What is the standard length of acrylic rod?

1000 mm and 2000 mm are the common stock lengths, with 3000 mm available in smaller diameters. Cut-to-length is standard and usually priced per cut, with a ±1 mm tolerance.

What tolerance can acrylic rod hold?

Extruded rod holds about ±0.1 mm at small diameters and ±0.3 mm at 30–60 mm. Cast rod holds roughly ±2 % of diameter, which is ±0.4 mm on a 20 mm rod. If you need tighter than extruded can hold, the practical route is to buy oversize and machine it.

Why does my 20 mm rod not fit a 20 mm hole?

Ovality plus tolerance. A 20 mm rod with ±0.2 mm diameter tolerance and 2 % ovality can measure 20.2 mm on one axis — which will not enter a true 20 mm hole. For a close fit, specify the rod undersize (for example 19.8 ± 0.1 mm) rather than nominal.

Is acrylic rod measured before or after cooling?

It should be measured after it has fully cooled and stabilised, because acrylic continues to shrink and to relax stress for some hours after production. A rod measured warm will read slightly large and may bow later.

Do I need to specify ovality and straightness?

Only if they matter to your application. For a decorative rod in a display, diameter and appearance are enough. For a rod that fits into a bore, or that spans a visible gap, ovality and straightness are the dimensions that decide whether it works — and neither is implied by a diameter tolerance.

Can I get a non-standard diameter?

Yes, but expect a minimum quantity and a lead time, because a mould tube or a die is dedicated to that size. In many cases it is cheaper to take the nearest standard size and machine it down, particularly in small quantities.

Send the drawing, or just the diameter and the application

We will tell you which process can hold your tolerance, flag anything on the drawing the process cannot deliver, and quote with ovality, straightness and end finish stated explicitly — so the goods-in inspection matches the purchase order.

Request a specification review

Ultimi messaggi

WhatsApp
Facebook
Twitter
LinkedIn
Pinterest
Ciao a tutti! Sono John, papà ed eroe di un bambino fantastico. Di giorno, sono un veterano dell'industria dell'estrusione della plastica che è passato dai reparti di fabbrica alla direzione tecnica. Sono qui per condividere ciò che ho imparato: cresciamo insieme!
it_ITIT

Chiedete un preventivo rapido

Inviare disegni e requisiti dettagliati via

Emial: [email protected]

Oppure compilate il modulo di contatto qui sotto: