Co-extruded cap layer peeling at the mitre: the bond failed at the merge, not in service

Real extruded plastic profiles and pipe on a production site
Real plastic profile extrusion production context. Photo: Pexels.

The problem

Symptom. A fabricator finds the 0.2 mm ASA cap lifting from a rigid PVC window profile after welding the corners, and rejects the whole batch as an adhesion failure.

What it costs. Delaminated lengths cannot be reworked, the welded frames have to be scrapped, and the dispute stalls a shipment until both parties test the same peel sample.

This guide ties peel strength to interface temperature at the merge, and gives the four checks that separate a cold cap melt from a bad compound.

Read the peel front before you blame the adhesive

A cap layer bonds only while both melts can interdiffuse at the merge. At a 155 °C interface the 0.2 mm ASA cap peeled at 0.8 N/mm and 78% of mitres failed 50 cycles; at 185 °C it held 2.9 N/mm and 3% failed.

Interface temp at merge (°C) Peel strength (N/mm) Mitres failing 50 cycles (%)
155 0.8 78
165 1.6 52
185 (specified) 2.9 3
205 (degraded) 2.7 4

Table 1 - Merge temperature against peel strength and thermal-cycle failures

Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.

Need a fixed price for this profile?

Send the cross-section drawing, material, cut length and annual volume. We will review die, calibration and tolerance, then return a written tooling and production quotation.

Get a profile quotationEmail [email protected]WhatsApp

Follow the interface back to the merge point

Typically, the causes were a cold cap melt, no compatibiliser, wet cap resin, a cap under 0.10 mm and a dirty die land. Check temperature first: a 25 °C gap between cap and core leaves a skin that never fuses.

A five-step diagnostic sequence

  1. Capture a peel sample first.
    Cut a 25 mm strip from the failed mitre and pull it at 180°; a continuous film at 0.8 N/mm points to the merge, not the adhesive.
  2. Measure both melt temperatures.
    Log cap and core melt at the merge; a difference over 10 °C means the colder skin never interdiffused.
  3. Check the interface temperature.
    Confirm 180 to 195 °C where the streams meet; below 170 °C peel strength falls under 1.5 N/mm.
  4. Verify cap thickness and dryness.
    A cap under 0.10 mm tears at the mitre, and wet resin leaves voids; dry the resin and reset the layer to 0.20 mm.
  5. Run the merge-temperature trial.
    Step from 155 to 205 °C and peel at each point; the 0.8 to 2.9 N/mm rise proves the bond was never formed.

The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

Co-extruded cap layer peeling at the mitre: the bond failed at the merge, not in service: calculated response trend and an illustrative root-cause split
Figure 1 — Calculated response trend and an illustrative root-cause split. Values are engineering guidance for diagnosis, not a measured survey; confirm them on your own line before changing a drawing or a specification.

Set the co-extrusion parameters that fuse the layers

Four settings hold the bond: a cap to core melt difference under 10 °C, an interface temperature of 180 to 195 °C, cap thickness of 0.15 to 0.30 mm, and a 180° peel strength above 2.5 N/mm. Below 170 °C it falls under 1.5 N/mm.

Parametro Typical target What goes wrong outside it
Cap / core melt difference at merge Under 10 °C A 25 °C gap leaves a cold skin that never fuses to the core
Interface temperature at merge 180-195 °C Below 170 °C peel strength falls under 1.5 N/mm
Cap layer thickness 0.15-0.30 mm Under 0.10 mm it tears at the mitre; over 0.40 mm it curls
180° peel strength Above 2.5 N/mm Under 2.0 N/mm the cap lifts after thermal cycling

Table 2 - Co-extrusion settings that fuse a 0.2 mm cap to PVC

Prove it with a merge-temperature trial

Run a merge-temperature trial with the compound fixed: step the interface from 155 to 205 °C and peel at each point. Strength rises 0.8, 1.6, 2.9 then 2.7 N/mm, so the peak near 185 °C and the fall at 205 °C bracket the window.

Field symptom Most likely cause Check that confirms it
Cap lifts as a continuous film Cold cap melt at the merge Interface thermocouple reads 155 °C instead of 185 °C
Peel starts only at cut ends Cap layer under 0.10 mm Micrometer shows 0.08 mm at the edge
Bond fails after summer heat No compatibiliser in the compound Peel strength drops below 2.0 N/mm after cycling
Random patches of delamination Wet cap resin or dirty die land Voids appear in the peel surface under magnification

Table 3 - Matching the peel pattern to the bond fault

Myth: "A process adjustment will fix it." Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.

Write the peel test into the purchase order

Write the peel test into the order: 180° peel strength, merge interface temperature, cap thickness and a retained reference sample. When both parties peel to the same method, a delamination claim becomes a number, not an opinion about the adhesive.

Need the section checked before tooling?

Send us the section and the installation conditions. We will review wall balance, tolerance and fixing detail, then return a marked-up drawing with a tooling quotation.

What to send us

  • Cross-section drawing with wall thicknesses
  • Material and colour
  • Installation temperature range
  • Fixing method and run length

Send the section drawing

What a fused cap saves over a warranty year

A fused cap is cheap insurance. A line welding 400 frames a day cannot rework a delaminated mitre; holding 185 °C keeps peel at 2.9 N/mm, while a 10 K drift can scrap a shift before the peel test is run.

Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.

Before you release this extruded profile

  • 180° peel strength and its test method are written into the order
  • Interface temperature at the merge is specified as 180-195 °C
  • Cap layer thickness and tolerance appear on the section drawing
  • A reference sample from the approved batch is retained by both parties
  • Thermal cycling of 50 cycles is agreed as an acceptance test

Write the measurement temperature and the tolerance into the drawing; most disputes are really about how the part was measured.

Why is my co-extruded ASA cap peeling off after welding?

The bond was probably never formed. If the interface sat at 155 °C instead of 185 °C, the cap melt was too cold to interdiffuse, giving peel strength near 0.8 N/mm rather than 2.9 N/mm.

Is this an adhesive or a material incompatibility problem?

Usually neither. Most field cases trace to the merge temperature or a missing compatibiliser. Check both melt temperatures first; a difference over 10 °C is the leading cause in typical cases.

What peel strength should a cap layer achieve?

Above 2.5 N/mm on a 180° peel test, with an interface of 180 to 195 °C. Below 2.0 N/mm the cap tends to lift after 50 thermal cycles from -10 to +60 °C.

Does cap thickness matter?

Yes. 0.15 to 0.30 mm is the working range. Under 0.10 mm the layer tears at the mitre; over 0.40 mm it curls from differential shrinkage and lifts at the corners.

Can I fix delamination by raising the die temperature?

Only within the window. Strength peaks near 185 °C and falls again by 205 °C as the polymer degrades. Step the interface in 10 K stages and peel at each rather than simply turning up the heat.

What should the acceptance test include?

A 180° peel strength figure, the merge interface temperature, cap thickness, a retained reference sample and 50 thermal cycles. Both parties then test the same method and the claim becomes a number.

Get a profile that holds its dimension

Send us the profile section, the length and the service conditions. We will review die, calibration and tolerance, then quote tooling and production with a defined measurement method.

To get an accurate quote, send:

  • Profile cross-section drawing
  • Material and colour
  • Cut length and annual volume
  • Service temperature and exposure

Request a profile quotation

Prefer to talk it through first?

Email [email protected] or message us on WhatsApp +86 177 1752 9949. Send a drawing, a sample or a specification and an engineer will reply.

Why buyers work with Uplastech

ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
it_ITIT

Chiedete un preventivo rapido

Inviare disegni e requisiti dettagliati via

Emial: [email protected]

Oppure compilate il modulo di contatto qui sotto: