LSR Injection Moulding: Metering, Mixing and the Needle Seal

Property retention against mix ratio error, and metering accuracy by pump type
A two percent ratio error costs about three percent of the properties, and a ten percent error costs thirty.

Why metering is the whole process

In thermoplastic injection moulding the material arrives ready to use. In LSR it arrives as two reactive components that have to be combined at a precise ratio, mixed intimately, and delivered to the mould before the reaction runs away. Every one of those three steps is a place where the process can fail, and all three are upstream of the cavity.

The ratio is the most sensitive. Platinum-catalysed addition cure needs the hydride crosslinker and the vinyl polymer in a stoichiometric balance, and the catalyst to drive it. A mixture that is rich in one component cures, but the network is wrong: the crosslink density is low, the tear strength drops, and the compression set rises. A mixture that is lean in catalyst cures slowly or not at all.

The property loss is steeper than most people expect. At a 2 percent ratio error the physical properties are about 97 percent of nominal, at 5 percent they are 88, at 10 percent they are 70 and at 20 percent they are 45. A 10 percent error is not a subtle degradation; it is a different material.

The pumps set the accuracy

Both components are pumped from drums by positive displacement pumps, and the accuracy of those pumps sets the ratio accuracy. Piston pumps hold about plus or minus 0.5 percent of dose, progressive cavity pumps about 1.5 percent, and peristaltic pumps about 3 percent.

Piston pumps are the standard for LSR because they meter a fixed volume per stroke, which is insensitive to viscosity. Their limitation is that they are cyclic: the dose arrives in pulses, and the machine has to smooth that into a continuous shot. Progressive cavity pumps deliver continuously and are simpler, but their output drifts as the stator wears, and the drift is different for part A and part B, which changes the ratio.

Pump type Akurasi Delivers Watch out for
Piston +/- 0.5 percent Discrete strokes Pulsation; needs a smoothing accumulator
Progressive cavity +/- 1.5 percent Berkelanjutan Stator wear changes the ratio over months
Peristaltic +/- 3 percent Berkelanjutan Tube wear and creep; used mainly for pigments

Table 1 — Metering pump types, their accuracy, and their failure mode.

The drift of a progressive cavity pump is the one that catches people out, because it is invisible. The machine holds the ratio it was set to, but the actual delivered volume changes as the stator wears, and part A and part B do not wear at the same rate. A line that ran perfectly for a year starts producing parts with a slight tackiness, and the cause is a worn stator rather than anything in the process settings.

Mixing: the static mixer is a consumable

Almost all LSR machines use a disposable static mixer: a plastic tube with a helical element that splits and recombines the flow. It has no moving parts, it costs a few euros, and it works extremely well until it does not.

The failure mode is gradual. Silicone cures slowly inside the mixer, starting at the walls where the material is oldest and warmest, and the cured layer narrows the passages. The pressure rises, the mixing quality falls, and eventually a slug of partially cured material is delivered into a cavity. The part has a soft, tacky region that may not be visible until it is flexed.

The discipline is to replace the mixer on a schedule rather than on failure. Every shift is typical for a busy line, every drum for a slow one, and always after any shutdown long enough for the material in the mixer to start curing. A mixer that has sat overnight is a mixer that should be replaced before the first shot.

A static mixer has a shelf life measured in hours once it is wet. The cost of replacing it early is a few euros; the cost of a slug of cured material in a medical part is a recall.

The needle seal

The needle seal is the valve between the cold runner and the cavity, and it is what allows LSR to be injection moulded at all. The material in the runner is liquid at 20 °C; the material in the cavity cures at 190. The needle has to open to let the shot in and close before the heat travels back up the sprue and cures the runner.

There are two arrangements. A needle valve uses a mechanical pin that seats into the gate, giving positive shut-off and clean gate break. An open drop relies on the material's own viscosity and the thermal balance to freeze the gate, which is simpler and cheaper but only works for small gates and short cycles.

The needle valve is the reason a 32 or 64 cavity LSR tool is practical. Each drop can be opened and closed individually, so the tool can be filled sequentially and every cavity sees the same pressure. With open drops, a large tool will not balance, and the outer cavities will be short or flash depending on where the thermal balance lands.

Fitur Needle valve Open drop
Shut-off Positive, mechanical Relies on the gate freezing
Gate quality Clean, small witness mark A tear-off that needs trimming
Cavity count Up to 64 or more Small tools only
Biaya Higher; each drop has a needle and an actuator Lebih rendah
Failure mode Needle wear or a stuck actuator Gate freeze inconsistent, so short shots or flash

Table 2 — Needle valve against open drop, and what each one costs you.

Needle wear is the maintenance item. The needle seats against a hardened gate insert, and after a few hundred thousand cycles the seat wears and the gate starts to flash. A worn needle is not repairable in place; the insert is replaced, and it is worth keeping a spare set for a production tool.

The metering faults that cause scrap

Symptom Likely cause Check
Soft, tacky patches Ratio error or an exhausted mixer Shot into a cup and inspect for homogeneity
Bubbles in the part Air entrained in dosing, or degassing off Vacuum level on both components, drum level, pump seals
Short shots on outer cavities Needle not opening fully, or a cold drop Needle stroke, and the temperature of the cold runner
Flash on one cavity only Worn needle seat at that drop Inspect the gate insert under magnification
Cure drifting over a shift Progressive cavity stator wear, or component temperature drift Component temperatures, and a ratio check with a scale

Table 3 — LSR metering faults, their causes and the first thing to check.

The ratio check with a scale is the simplest diagnostic and the most under-used. Dispense a fixed number of shots into two cups with the needle closed, weigh them, and compare the masses against the expected ratio. It takes five minutes and it separates a metering problem from a moulding problem definitively.

Maintenance that keeps the ratio honest

An LSR line rewards a maintenance schedule more than almost any other process, because most of its failure modes are gradual and invisible. The following four items cover most of the risk.

  1. Replace the static mixer on a fixed schedule and after every shutdown.
  2. Check the ratio by weight weekly, and log it, so that drift is visible as a trend rather than as a defect.
  3. Inspect the needle seats at a fixed interval, and replace the gate inserts as a set rather than one at a time.
  4. Verify the component temperatures, because viscosity changes with temperature and a dose that is volumetric will deliver a different mass if the component is cold.

The fourth item is the subtle one. A volumetric pump delivers a fixed volume, and if the component is 5 °C cooler its density is higher, so the mass delivered is higher and the ratio shifts. That is why the drums are usually temperature controlled and why a line that runs cold first thing in the morning can produce different parts from the same settings in the afternoon.

How accurate does the LSR mix ratio need to be?

Within about 2 percent to keep the physical properties within 3 percent of nominal. At 10 percent error the properties are down about 30 percent, which is a different material.

Which pump is best for LSR?

Piston pumps, at about plus or minus 0.5 percent of dose. Progressive cavity pumps are simpler but drift as the stator wears, and peristaltic pumps are used mainly for pigments.

How often should the static mixer be replaced?

Every shift on a busy line, every drum on a slow one, and always after a shutdown long enough for material to start curing inside it.

What is a needle seal for?

It shuts off the gate between the cold runner and the hot cavity, so the shot goes in and the runner stays liquid. Without it, heat travels back up the sprue and cures the runner.

Why do outer cavities go short?

Usually a needle that is not opening fully, or a cold drop. With open drops instead of needle valves, a large tool simply will not balance.

Why do parts get tacky over a shift?

Either an exhausted mixer or a ratio drift. Progressive cavity stators wear, and component temperature changes alter the delivered mass even when the volume is correct.

Setting up an LSR line or chasing scrap?

Send the part, the volume and the current scrap rate. We will tell you whether the metering, the mixing or the needle seal is the constraint, and what the tool needs.

Talk to a silicone engineer

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
id_IDID

Minta Penawaran Cepat

Kirim gambar dan persyaratan terperinci melalui