Falling Output on a PE Pipe Line: Reading Screw Wear

Falling Output on a PE Pipe Line: Reading Screw Wear
Profile extrusion: a production part is the only useful reference for a discussion about process drift.

When the same screw speed delivers less pipe per hour and melt temperature creeps up, the screw-to-barrel clearance has likely grown.

What the failure looks like on the line

PE pipes and profiles are tolerant in service but unforgiving in cooling, where slow crystallisation keeps changing the section after sizing.

A PE pipe line needs a higher screw speed each month to hold the same output and metre weight, while melt temperature and motor load rise at unchanged heater settings. The change is gradual and is often mistaken for a raw-material or formulation drift.

Wear opens the flight-to-barrel clearance, so material leaks back over the flights instead of being conveyed forward; the pumping efficiency falls and more shear heat is generated per kilogram. The line compensates by raising screw speed, which further increases melt temperature and can narrow the processing window. Measuring output per revolution, rather than screw speed alone, exposes the loss early.

The useful question is not whether the part conforms, but which condition was never written into the specification. On a buyer's specification this distinction matters: a part can measure inside tolerance and still fail in use, because the drawing records geometry while the complaint records behaviour. Screw-to-barrel clearance is usually the first value both sides compare, and it is also the one most often quoted without the conditions attached to it.

The process window that decides it

Four variables move this result more than the rest. The ranges below are illustrative engineering guidance for a first discussion; confirm them on your own tool, material grade and part geometry before they become contract terms.

Variable Typical window What fails outside it
Screw-to-barrel clearance 0.1-0.3 mm (new tool) Doubling the clearance markedly reduces drag-flow pumping efficiency
Specific output within +/- 10 % of baseline A falling kg/h per rpm is the earliest sign of wear
Melt temperature at die 190-215 C A steady upward drift at fixed settings points to added shear heat
Drive motor load 60-80 % of rated Rising load at lower output signals wasted shear, not useful pumping

Table 1. Starting window for a joint process trial. Values are engineering guidance, not a measured survey.

Screw-to-barrel clearance is typically held at 0.1-0.3 mm (new tool). Doubling the clearance markedly reduces drag-flow pumping efficiency Record it together with the measurement point and the moment in the cycle; a single number without a location is not a process setting.

Specific output is typically held at within +/- 10 % of baseline. A falling kg/h per rpm is the earliest sign of wear When this drifts, the symptom usually appears at one cavity, one sheet position or one lane before it appears across the whole batch.

Melt temperature at die is typically held at 190-215 C. A steady upward drift at fixed settings points to added shear heat A change here is cheap during a trial and expensive after tooling release, so treat it as a controlled variable with a documented re-approval.

Drive motor load is typically held at 60-80 % of rated. Rising load at lower output signals wasted shear, not useful pumping Put it on the change-control list, otherwise an unannounced material or setting substitution will be mistaken for ordinary process noise.

Reading the response curve

Falling Output on a PE Pipe Line: Reading Screw Wear: Output rate (% of nominal, relative) against Screw service time (kh)
Figure 1. Left: Output rate (% of nominal, relative) against Screw service time (kh). Right: how audited failures of this type typically split by cause. All plotted values are illustrative engineering guidance, not a measured survey.

The left panel shows output rate (% of nominal, relative) as screw service time (kh) increases: the response falls from 98 to 38 on the illustrative 0–100 scale. The dashed line at 80 marks a proposed acceptance limit, not a universal standard. Move that line only after the test method and the sample plan have been agreed, otherwise two suppliers can both be compliant and still deliver different parts.

Read the shape rather than a single point. A curve that changes quickly near the limit is more sensitive to ordinary process noise than one that approaches it gradually, and that difference should be reflected in how tightly the setting is controlled and how often it is checked.

Where the causes actually sit

The right panel of Figure 1 splits audited failures of this type into five groups. The percentages are illustrative engineering guidance for prioritising an investigation, not a measured survey and not a prediction for your line.

Cause Illustrative share First check
Flight-to-barrel wear 38% Trend kg/h per rpm rather than absolute output against screw speed.
Abrasive filler or regrind 22% Record melt temperature and motor load at a fixed, reference setpoint.
Corrosive degradation products 16% Measure flight diameter and barrel bore at the next planned shutdown.
Rising screw speed compensation 14% Compare current specific output with the commissioning baseline.
Blocked screen pack misread 10% Rule out a screen-pack blockage before attributing the loss to wear.

Table 2. Cause split and the corresponding first check. Shares are indicative and sum to 100.

Flight-to-barrel wear accounts for roughly 38% of the illustrative split. Trend kg/h per rpm rather than absolute output against screw speed. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.

Abrasive filler or regrind accounts for roughly 22% of the illustrative split. Record melt temperature and motor load at a fixed, reference setpoint. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.

Corrosive degradation products accounts for roughly 16% of the illustrative split. Measure flight diameter and barrel bore at the next planned shutdown. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.

Checks before sign-off

Work through these in order; measuring a later variable before an earlier one hides the cause rather than finding it.

  1. Trend kg/h per rpm rather than absolute output against screw speed.
  2. Record melt temperature and motor load at a fixed, reference setpoint.
  3. Measure flight diameter and barrel bore at the next planned shutdown.
  4. Compare current specific output with the commissioning baseline.
  5. Rule out a screen-pack blockage before attributing the loss to wear.

Keep a retained reference sample beside every result. When a batch is disputed, the comparison that settles it is almost always between the retained part and the current one under the same method, not between either part and a number on a drawing. Record the instrument, the operator, the conditioning time and the position on the part or sheet for each reading.

Writing it into the specification and the evidence pack

Specific output shall stay within the agreed band of the commissioning baseline at the reference setpoint, with screw and barrel clearances recorded at each planned inspection.

Write the requirement as a behaviour at a stated condition, not as a brand of material or a machine setting. State the test method, the conditioning, the sample plan and the rule for deciding a pass. Where a document is needed, ask the supplier for documentation that covers the actual construction and check its scope against your own market before approval; a document for the base material alone does not describe the finished part you are buying.

At first-article approval, freeze the drawing revision, the material and colour identification, the process window, the tool and cavity identification, and the inspection method. Any later change to grade, site, tool, or window should trigger a new first article rather than a paper waiver. Keep retained samples from the approved lot and from each production lot so that a future comparison is possible.

Evidence item What it must show
Approved drawing and revision The exact geometry and tolerances the decision applies to
Material and colour identification Grade, supplier, colour reference and any declared recycled content
Process window and change log The agreed settings and any deviation since approval
Inspection record and retained samples Method, conditions, results and a physical reference from the same lot

Table 3. Minimum evidence pack for a first-article decision and a later batch dispute.

The values quoted here are illustrative engineering guidance, not a measured survey. Agree the test method, the sample size and the acceptance rule before comparing numbers across suppliers.

Questions buyers ask

Is this a material problem or a process problem?

Wear opens the flight-to-barrel clearance, so material leaks back over the flights instead of being conveyed forward; the pumping efficiency falls and more shear heat is generated per kilogram. The line compensates by raising screw speed, which further increases melt temperature and can narrow the processing window. Measuring output per revolution, rather than screw speed alone, exposes the loss early. It is worth separating the two before a supplier changes a grade: hold the material constant for one controlled run, then move one setting at a time. If the symptom follows the setting, the material was never the cause.

Can screw-to-barrel clearance be traded against cycle time?

Only within the window stated in Table 1, and only with a recorded trial. Doubling the clearance markedly reduces drag-flow pumping efficiency A faster cycle that sits outside the window usually moves the failure downstream, where it costs more to find.

What should be recorded at incoming inspection?

Keep the measurement, the method, the sample identity and the conditions together. Trend kg/h per rpm rather than absolute output against screw speed. A result without its conditions cannot be compared with a later batch.

Does a change of PE require re-approval?

Treat any change to material grade, tool, site or process window as a change that needs a new first-article decision. For profile extrusion work the drawing alone is not enough; the process route is part of what was approved.

How many samples are enough for a first-article decision?

There is no universal number. Sample across cavities, lanes, sheet positions or reel lengths so that the spread is visible, not just the average. Agree the sample plan and the acceptance rule with the supplier before the trial starts.

What belongs in the evidence pack?

The approved drawing and revision, the material and colour identification, the process window, the inspection method and results, the retained reference samples, and documentation covering the actual construction. Ask the supplier to state the scope of each document and check it against your own market.

Seeing this on a current profile extrusion job?

Send the drawing, the material and grade, the process window you are running, and the point in the cycle or the shelf life where the fault appears. We will help you separate a material question from a process question and a specification question before anyone changes a tool.

Talk to our profile extrusion team

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
fr_FRFR

Demander un devis rapide

Envoyer les dessins et les exigences détaillées via