Packing Pressure and Hold Time: How to Set Them From the Part

Chart of cavity pressure against time showing gate freeze point and the effect of different hold times on part weight
Cavity pressure rises during filling, drops at the switchover, then holds flat while the gate is open. The moment it starts to fall is gate freeze — and it is the only correct hold time.

What packing actually does

When the screw stops, the cavity is full but the part is not finished. The polymer is cooling and shrinking, and that shrinkage has to be made up with more material — otherwise the part pulls away from the cavity walls, sinks, and ends up underweight and undersized.

Packing pressure does that make-up. It pushes additional melt through the still-open gate to compensate for shrinkage. Hold time is how long that pressure is maintained. Both are set by the part, not by preference, and both have an exact correct answer that can be measured.

The single most useful measurement in injection moulding: cavity pressure at the gate. It rises through filling, drops when the machine switches from velocity to pressure control, holds flat while the gate is open, and then falls when the gate freezes. That falling edge is gate freeze, and it is where hold time should end.

The three phases of packing

Phase What happens Time scale Controlled by
Filling Cavity fills, pressure rises 0.5 – 3 s Injection velocity profile
Compression / switchover Velocity control hands over to pressure control; peak cavity pressure 0.1 – 0.5 s Switchover point and pack pressure setting
Packing / holding Additional melt enters through the gate to offset shrinkage 2 – 20 s Hold pressure and hold time
Gate freeze Gate solidifies; no more material can enter — Gate geometry and cooling
Refrigeración Part cools with no further mass change Until ejection Tiempo de enfriamiento

Table 1 — The phases of a cycle after filling. Everything after gate freeze is cooling, and extending hold beyond gate freeze does nothing except waste time.

Gate freeze is the pivot. Before it, hold pressure controls part weight and dimensions. After it, hold pressure has no effect at all, because there is no path for material to enter. Running hold time past gate freeze is the most common wasted second in injection moulding.

Finding gate freeze

There are two ways: with a cavity pressure sensor, and without one. The sensor method is faster and more accurate; the weight method works on any machine.

With a sensor. Plot cavity pressure against time. The pressure holds flat during packing and then drops when the gate freezes and the part starts to shrink away from the sensor. The time at which the drop begins is gate freeze.

Without a sensor. Run a series of parts at increasing hold times, weighing each one. Part weight rises with hold time and then plateaus. The point where the curve flattens is gate freeze. It takes six to eight parts and about twenty minutes, and it needs no instrumentation.

Hold time (s) Part weight (g) Interpretation
1.0 24.82 Short — sink likely
2.0 25.31 Still filling out
3.0 25.64 Approaching plateau
4.0 25.78 Near plateau
5.0 25.81 Plateau
6.0 25.82 Plateau — gate frozen at ~5 s
8.0 25.82 No change; 3 s wasted

Table 2 — The weight-plateau method. Gate freeze is where the weight stops changing, which here is about 5 seconds. Hold time should be set at 5 seconds, not 8.

The plateau method has one subtlety: it must be run at the intended pack pressure. At a low pack pressure the gate may freeze earlier because less hot melt is flowing through it; at a high pack pressure the gate stays open longer. Set pack pressure first, then find gate freeze.

Setting pack pressure

Pack pressure is expressed as a percentage of injection pressure on most machines, which makes it machine-specific and not portable between presses. The useful number is cavity pressure, and the useful target is a part that is dimensionally correct and visually acceptable.

Pack pressure Effect on part Symptoms
Too low Insufficient material added Sink, voids, short shots, undersize, warpage
Correct Weight at plateau, dimensions on nominal None
Too high Over-packed; stress and flash Flash, ejection damage, high residual stress, warpage in the other direction

Table 3 — Pack pressure effects. Both too low and too high cause warpage, which is why warpage alone does not tell you which way to go.

The practical procedure is to start at a pressure that clearly produces a short shot or visible sink, then raise it in steps until the part is dimensionally correct and cosmetically acceptable, then check for flash. The correct setting is the lowest pressure that produces an acceptable part — not the highest that does not flash.

Running at the lowest acceptable pressure matters because higher pack pressure means higher residual stress, which means more warpage and more stress cracking later. It also means more clamp force required and more wear on the tool.

Packing profiles

Single-stage packing is fine for simple parts. For parts with thick sections, ribs or a long flow path, a two-stage or three-stage profile gives better results.

Perfil Forma Utilice
Single stage Constant pressure throughout hold Simple, uniform-wall parts
Two stage (high then low) High pressure briefly, then reduced Parts with a thick section that must be packed before the gate freezes
Three stage High, medium, low Thick parts with a long hold; reduces stress at the gate
Ramp down Gradual decay Reduces gate stress marks; used on optical parts

Table 4 — Packing profiles. The two-stage profile is the most common upgrade: it packs the thick section early while the gate is open, then reduces pressure to avoid over-packing the thin sections.

The reason for reducing pressure later is that thin sections freeze first. Once they are solid, additional pressure cannot pack them, but it still acts on the gate area and on the still-molten core of thick sections. A high pressure held too long over-packs the gate region, which shows as a stress halo around the gate and sometimes as a small crack.

How the resin changes the numbers

Resin Typical gate freeze Pack pressure (cavity) Notas
PP 2 – 4 s 200 – 400 bar High shrinkage; needs generous packing
PE 2 – 5 s 200 – 400 bar Similar to PP
PS 2 – 4 s 200 – 350 bar Low shrinkage; less critical
ABS 3 – 6 s 300 – 500 bar Moderate; watch gate stress
PC 4 – 8 s 400 – 700 bar High viscosity; needs high pressure
PA66 2 – 4 s 400 – 800 bar Crystalline; freeze is fast once it starts
POM 3 – 6 s 400 – 700 bar High crystallinity; significant shrinkage
PBT 2 – 4 s 400 – 700 bar Fast freeze; short packing window

Table 5 — Typical packing values by resin. The gate freeze times assume a 1.5–2 mm gate; a bigger gate stays open longer.

Gate size is the strongest influence on freeze time, and it is fixed in the tool. A 1 mm gate on a 3 mm wall freezes in about a second, which leaves almost no packing window and produces sink no matter what the machine does. That is a tooling problem, and no process setting fixes it.

Diagnosing from the part

Defecto What it suggests First adjustment
Sink on a thick section Gate froze before the section was packed Longer hold, higher pressure, or a bigger gate
Voids inside a thick section Same as sink, but the skin is stiff enough to hold Same; also check for moisture
Flash at the parting line Pack pressure too high or clamp force too low Reduce pressure; check clamp tonnage
Alabeo Either over- or under-packed Check part weight against the plateau; then adjust
Stress halo at the gate Over-packed, or pressure released too fast Profile the pressure down; slow the release
Short shot at the end of flow Insufficient pressure, or gate froze early Raise pressure; check melt temperature
Weight variation between shots Inconsistent switchover or check-ring leakage Check switchover repeatability and non-return valve

Table 6 — Reading the part for packing problems. Weight variation is the most diagnostic: a stable process produces parts within 0.2% of each other.

Part weight is the single best production indicator of packing stability. If the weight varies by more than about 0.3% between shots on a stable process, something is changing — switchover position, melt viscosity, or check-ring leakage. Weighing ten parts once an hour catches most packing problems before they become a customer complaint.

How do I find the right hold time?

Weigh parts at increasing hold times. The weight rises and then plateaus; the point where it flattens is gate freeze, and that is the correct hold time. With a cavity pressure sensor, watch for the pressure to start falling — same answer, faster.

What happens if hold time is too short?

The gate freezes before the part is fully packed. The result is sink on thick sections, internal voids, undersized dimensions and warpage. Short hold time is the most common cause of sink that appears "for no reason" on a part that used to run fine.

What happens if hold time is too long?

Nothing to the part, but you lose cycle time. Once the gate is frozen no more material can enter, so additional hold time has zero effect. On a 20-second cycle, running hold 3 seconds past gate freeze costs 15% of output for no benefit.

Should pack pressure be higher or lower than injection pressure?

Lower, typically 40–70% of injection pressure. Injection pressure is what it takes to fill the cavity at the required velocity; pack pressure only needs to compensate for shrinkage. Running pack at full injection pressure over-packs the part and causes flash.

Why does my part warp in one direction and sink in another?

Because different sections are packed differently. Thin sections freeze early and cannot be packed; thick sections stay open longer and receive more material. The differential shrinkage between them causes warpage. A packing profile or a wall-thickness change is the fix.

Does gate size affect packing?

Strongly. A larger gate stays molten longer, which gives a longer packing window and better sink control. A gate that freezes in under a second leaves almost no window. If a part cannot be packed, gate size is often the real problem.

How do I know if the check ring is leaking?

Part weight becomes inconsistent between shots, and the cushion (the amount of melt left in front of the screw at the end of hold) varies. A leaking check ring lets material flow back during packing, so the effective pack pressure is lower and variable.

Is cavity pressure control worth installing?

For high-volume precision parts, yes — it makes the process independent of material viscosity variation. For general purpose work, the weight-plateau method gives you the same information once, and hourly weighing maintains it.

Parts sinking, warping or varying in weight?

Send us the part drawing, the resin, the gate size and your current pack settings. We will tell you whether the limit is the process or the tool, and what the correct hold time is for that gate.

Talk to a moulding engineer

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
es_ESES

Solicite un presupuesto rápido

Envíe los planos y los requisitos detallados a través de

Emial: [email protected]

O rellene el siguiente formulario de contacto: