PC Injection Molding: Drying, Melt Temperature and Stress Cracking

Clear polycarbonate injection moulded lens cover and an opaque black PC bracket on an inspection bench
A clear PC cover and a glass-filled black PC bracket from the same family of grades. The transparent part is where every PC problem becomes visible at once: flow marks, stress, and any moisture the dryer missed.

Why PC is difficult, and why it is worth it

Polycarbonate has an unusual combination: it is transparent, it has an impact strength of 600 – 900 J/m notched, it holds its properties to 120 °C, and it is dimensionally stable. Nothing else in the commodity engineering range does all four. That is why it is used for machine guards, lenses, medical housings, electrical enclosures and power-tool bodies.

The price of that combination is a narrow processing window and two failure modes that are unforgiving. PC must be dried to below 0.02 % moisture — one of the tightest limits of any common polymer — and it must be moulded with low residual stress, because polycarbonate stress-cracks in contact with almost every solvent it meets, including some mould releases, some adhesives, and some cleaning agents.

The two numbers that decide whether a PC job runs: moisture below 0.02 % at the hopper, and residual stress low enough to survive a 30-second immersion in carbon tetrachloride or a suitable stress-crack test. Get both right and PC is straightforward. Get either wrong and you will spend weeks chasing a defect that is not where it appears.

Grades

Grade family Key property MFR (g/10 min) Used for
Optical / lens Haze < 1 %, low birefringence 6 – 15 Lenses, light covers, display windows
General purpose Balanced clarity and flow 10 – 22 Housings, guards
High flow Thin walls, long flow 22 – 40 Thin-wall electrical parts
Flame retardant UL94 V-0 at 1.5 mm 8 – 20 Power supplies, chargers
UV stabilised Retains clarity outdoors 8 – 18 Outdoor lenses, signage
Scratch resistant (hard coat) Surface hardness 2 – 3 H 8 – 15 Touch screens, displays
Glass filled, 10 – 30 % Modulus 6 – 10 GPa 5 – 15 Structural brackets
PC/ABS blend Better flow, lower cost 10 – 25 Housings where clarity is not needed
Medical / ISO 10993 التوافق الحيوي 8 – 20 Device housings, fluid paths

Table 1 — PC grade families. Optical grades are a separate specification, not a premium version of general purpose.

Drying: the non-negotiable step

Polycarbonate hydrolyses. Water at moulding temperature breaks the carbonate linkage, reducing molecular weight permanently. A single wet shot does not just produce a cosmetic defect — it degrades the material, and the part that comes out has lower impact strength even after the streaks are gone.

Moisture content Visual result Impact retention
< 0.015 % Clear, no streaks 100 %
0.02 % Clear on most parts 95 – 100 %
0.03 % Faint silver streaking near the gate 85 – 95 %
0.05 % Visible streaks across the part 70 – 85 %
0.10 % Bubbles, splay, cloudy patches 50 – 70 %
0.20 % Gross foaming, unusable < 40 %

Table 2 — PC moisture versus outcome. The impact loss is permanent and invisible.

Dryer type درجة الحرارة Time الملاحظات
Desiccant wheel (recommended) 120 °C 3 – 4 h Dew point −20 °C or lower; the standard for PC
Vacuum dryer 110 – 120 °C 1.5 – 2.5 h Faster; good for small batches
Hot air oven 120 °C 4 – 6 h Only if the air is genuinely dry; ambient humidity re-wets the resin
Hopper dryer, short 120 °C 2 h minimum Not sufficient for a cold-start; only for holding dried resin

Table 3 — Drying routes. A hot-air oven in a humid climate can plateau at 0.05 % and never get lower.

Myth: "the streaks disappeared after an hour, so it's fine now." Silver streaks disappear when the surface moisture drops below about 0.03 %. The molecular weight damage from the first wet shots remains in the barrel until it is purged, and the parts made in that period have reduced impact. Purge and restart after a moisture event — do not just wait for the streaks to go.

The processing window

المعلمة Typical setting الملاحظات
درجة حرارة الذوبان 280 – 310 °C Below 270: unmelt and high stress. Above 320: degradation and yellowing
Barrel profile 260 / 280 / 295 / 300 °C Feed zone cool to avoid bridging
Nozzle 290 – 300 °C Use a reverse-taper or free-flow nozzle
Mould temperature 80 – 110 °C The single biggest lever on stress and surface
Injection pressure 80 – 140 MPa High viscosity; expect high pressures
Injection speed Moderate to fast Fast fill reduces stress but can cause jetting
Hold pressure 50 – 70 % of injection Long hold; PC packs slowly
Back pressure 0.5 – 1.5 MPa Helps homogenise; watch for over-heating
سرعة اللولب 40 – 70 rpm Low peripheral speed
Residence time < 8 min Long residence at 300 °C yellows the melt
Regrind 0 – 20 % Must be dried again; each pass reduces molecular weight

Table 4 — A starting window for optical-grade PC. Confirm against the grade datasheet.

Mould temperature is where most PC problems are solved or created. At 60 °C a PC part looks fine and is full of frozen-in stress: it will craze around inserts, crack when assembled, and fail a solvent test. At 90 – 100 °C the surface replicates better, the stress relaxes before the part ejects, and the cycle is longer but the yield is far higher. The extra 10 seconds per shot is almost always cheaper than the sorting.

Residual stress: how to see it and how to remove it

Test الطريقة Pass criterion
Solvent immersion Carbon tetrachloride or a proprietary stress-crack reagent, 30 s to 3 min No crazing within 60 s
Solvent wipe Wipe with acetone or ethyl acetate, leave 5 min No crazing
Polarised light View between crossed polarisers Uniform low-order colour; strong bands indicate stress
Heat relaxation Measure, hold at 120 °C for 1 h, re-measure Dimensional change < 0.2 %
Assembly test Torque the screw to specification, hold 24 h No cracking at the boss

Table 5 — PC stress tests. The solvent immersion test is the industry standard and takes one minute.

Annealing removes stress after the fact and is standard practice for machined or heavily loaded PC parts. For moulded parts it is a band-aid: the right fix is a hotter mould, a slower fill and better packing.

Annealing schedule درجة الحرارة Time
Thin parts, < 2 mm 120 °C 1 h
2 – 4 mm 120 °C 2 h
4 – 8 mm 120 °C 3 – 4 h
Glass filled 125 °C 2 – 4 h
Cool-down rate — ≤ 10 °C/h to avoid re-introducing stress

Table 6 — Annealing. Slow cooling matters as much as the hold time.

Design rules

الميزة Rule Why PC is different
Wall thickness 2.0 – 3.5 mm; avoid < 1.5 mm High viscosity makes thin walls hard to fill
Wall uniformity Within 20 % Thick sections cause voids and stress
Internal radius ≥ 0.5 × wall, preferably 1.0 × PC is notch sensitive — sharp corners are crack starters
Draft 1.5° minimum High shrinkage force; parts grip the core
Gate Large, edge or direct; avoid small pin gates High shear degrades PC at the gate
Metal inserts Design for 0.3 – 0.5 % differential expansion PC expands 65 – 70 × 10⁻⁶/K vs 23 for aluminium
Threads Moulded threads only in low-stress areas Thread roots are stress concentrators
Snap fits Strain ≤ 1.0 % for repeated flexing PC tolerates a single snap better than repeated
Sharp edges Break all external edges 0.3 mm Handling damage becomes a crack

Table 7 — PC design rules. Notch sensitivity is the theme.

Optical parts: the extra requirements

A lens or a light guide is a different specification from a housing, and the differences are not obvious from a datasheet.

Requirement What it needs If it is missed
Tool polish SPI A-1 or A-2, diamond polish Every tool mark is visible in the transmitted light
Gate location Outside the optical aperture Gate mark and flow lines in the field of view
Flow front Single, uninterrupted front Weld lines visible as a bright or dark line
Mould temperature 100 – 120 °C Flow marks and internal stress birefringence
Material grade Optical grade, low birefringence Rainbow patterns in polarised light
Drying 0.01 % or better Micro-bubbles that scatter light
Packing Low hold pressure, slow Orientation and birefringence at the gate
Handling No contact with the optical surface Scratches that cannot be polished out

Table 8 — Optical PC requirements. Birefringence is the one that is invisible until the part is between polarisers.

Defects and causes

العيب السبب Fix
Silver streaks / splay Moisture Dry to 0.02 %; check dew point and hopper seal
Crazing after assembly Residual stress plus solvent or stress Raise mould temperature; anneal; check assembly torque
Yellowing Over-temperature or long residence Lower melt 10 °C; reduce shot-to-barrel ratio
Flow marks on clear parts Cold mould or slow fill Mould to 100 °C; increase injection speed
Bubbles in thick sections Voids from shrinkage, or moisture Increase hold pressure and time; dry
Weld line visible Low mould temperature, slow front Raise mould; raise speed through the weld
Crack at the gate High shear, small gate Enlarge the gate; slow the first stage
Cloudy patches Moisture or degraded material Dry; purge; check for dead spots in the hot runner
Black specks Carbonised material in the hot runner or nozzle Purge with PC purge compound; inspect hot-runner tips

Table 9 — PC defects. Note that four of the nine trace back to moisture or residence time.

Flow length, wall thickness and the pressure ceiling

PC has high melt viscosity, which limits how far it can flow through a thin wall before the pressure runs out. This is the constraint that most often forces a design change, and it is worth checking before the tool is cut.

Wall thickness Practical flow length (unfilled PC) Flow ratio
1.0 mm 70 – 90 mm 70 – 90 : 1
1.5 mm 130 – 170 mm 85 – 115 : 1
2.0 mm 200 – 260 mm 100 – 130 : 1
2.5 mm 280 – 360 mm 110 – 145 : 1
3.0 mm 360 – 450 mm 120 – 150 : 1
4.0 mm 480 – 600 mm 120 – 150 : 1

Table 9 — Flow length for unfilled PC at 300 °C melt and 100 °C mould. Glass-filled grades reach 60 – 75 % of these figures.

If the required flow length exceeds the table, you have four options: thicken the wall, add a gate in the middle, raise the melt temperature (limited by degradation), or change material. Adding a second gate is often the cheapest, but it creates a weld line — which on a transparent part is a visible defect and must be placed outside the optical area.

The wall-thickness trap: designers often thin a PC wall to save material and cycle time, then find the part will not fill. Going from 2.5 mm to 2.0 mm cuts the part volume by 20 % but cuts the flow length by nearly 30 % and raises the required injection pressure by 50 – 70 %. On PC the two effects usually cancel out and the part fails to fill at the pressure limit.

Medical and food-contact PC

Polycarbonate is widely used in medical devices, and the qualification requirements are specific.

Requirement What it means Watch out for
ISO 10993 Biocompatibility for the intended contact duration The grade, not the polymer, is qualified
USP Class VI Biological reactivity Often quoted instead of ISO 10993 — they are not equivalent
Gamma sterilisation 25 – 50 kGy PC yellows slightly; specify a gamma-stable grade
EtO sterilisation Ethylene oxide Requires aeration time; PC absorbs EtO
Autoclave 121 – 134 °C steam PC is marginal — 20 – 50 cycles before crazing
Food contact, EU EU 10/2011 BPA migration limits apply; check the grade's declaration
Food contact, US FDA 21 CFR 177.1580 Grade-specific

Table 10 — PC medical and food qualification. Autoclave is the requirement that usually rules PC out.

The BPA point is worth stating plainly: polycarbonate is made from bisphenol A, and BPA is restricted in food-contact applications for infants in the EU and has been voluntarily withdrawn from baby bottles in many markets. For food-contact PC in any infant-related application, expect a regulatory conversation. For medical device housings and industrial lenses, PC remains standard.

Inspecting a transparent part

العيب How to see it Accept / reject basis
Flow marks Hold at an angle to a light source Any visible mark in the optical aperture is a reject
Weld line Backlight, viewed through the part Reject in the aperture; acceptable outside
Birefringence Crossed polarisers Compare against a limit sample
Micro-bubbles 10× loupe under raking light Any bubble in the aperture is a reject
Gate mark Direct inspection Outside the aperture by design
Scratches Raking light Handling damage — reject
Haze Haze meter Per the drawing; typically < 1 % for optical

Table 11 — Transparent part inspection. Crossed polarisers are the only way to see birefringence.

Note that three of these checks need equipment that a general inspection bench does not have: polarisers, a haze meter and a controlled light source. A supplier who says they can mould optical PC should be able to show you all three.

Frequently asked questions

Can PC be moulded without a desiccant dryer?

Not reliably. PC needs 120 °C of dry air at a dew point of −20 °C or better. A hot-air oven in a humid factory stabilises around 0.05 – 0.1 %, which produces streaked, weakened parts. If you do not have a desiccant dryer, you cannot run PC.

Why does my PC part crack a week after moulding?

Residual stress plus a solvent. The two usual solvents are a mould release agent (silicone or a solvent carrier) and an assembly adhesive or cleaning fluid. Stress cracking is delayed because the solvent needs time to diffuse. Run the solvent immersion test on a moulded part — if it crazes within 60 seconds, the moulding is over-stressed.

What is the maximum wall thickness for PC?

Practically 4 – 5 mm. Beyond that, the core stays molten while the skin freezes and you get voids and internal stress that annealing will not fully remove. For thick sections, consider a different material or a two-piece design.

Can PC be ultrasonically welded?

Yes, but it needs more energy than ABS and the joint design matters more. Amorphous PC welds well with a step joint and a generous energy director. Glass-filled PC is much harder — the fibres interfere with the melt at the interface.

How much does PC shrink?

0.5 – 0.7 % for unfilled, 0.2 – 0.5 % for 20 – 30 % glass filled. The unfilled figure is more sensitive to mould temperature and wall thickness than ABS, so the tool needs to be corrected against parts moulded at production conditions, not at a trial setting.

Is PC suitable for outdoor use?

Standard PC yellows under UV within 1 – 2 years. UV-stabilised grades with a coextruded or coated UV cap last 5 – 10 years. For anything with a service life requirement outdoors, specify the UV grade and consider a hard coat as well.

What causes a cloudy patch on a clear PC part?

Usually moisture that was trapped in a slow-filling area, or degraded material from a hot-runner dead spot. If the cloudiness is always in the same place, suspect the hot runner; if it moves, suspect moisture.

PC or PMMA for a lens?

PMMA has better optical clarity and UV resistance and is cheaper; PC has 10 – 20× the impact strength and better heat resistance. For a lens that will be dropped, PC. For a lens that must be optically perfect and will be treated carefully, PMMA. For a lens that must do both, PC with a hard coat.

Moulding a PC part and fighting stress or clarity?

Send the drawing and the failure mode. We will tell you whether it is a drying problem, a mould-temperature problem or a design problem — and which of the three is cheapest to fix.

Talk to a PC moulding engineer

أحدث المنشورات

واتساب
فيسبوك
تويتر
لينكد إن
بينتيريست
Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
arAR

اطلب عرض أسعار سريع

إرسال الرسومات والمتطلبات التفصيلية عبر

Emial: [email protected]

أو املأ نموذج الاتصال أدناه: