A 6 m cooling tank with a 10 K split from top to bottom: the profile is leaving too hot

Real extruded plastic profiles and pipe on a production site
Real plastic profile extrusion production context. Photo: Pexels.

The problem

Symptom. During commissioning a buyer logs 24 °C water at the top of a 6 m cooling tank and 14 °C at the bottom, and the extruded PVC profile still reads 45 °C at the tank exit.

What it costs. The line cannot be signed off, and the resulting length scatter and post-extrusion warp are blamed on the die while the tank design is the real gap.

This guide links stratification to recirculation flow and baffles, and gives the four measurements that settle a commissioning dispute.

Measure the tank at three depths before you blame the die

Warm water rises, so an unbaffled 6 m tank forms a stagnant top layer. At 100 L/min we logged 24 °C at the surface against 14 °C at the bottom, a 10 K split, and the profile left at 45 °C rather than 32 °C.

Recirculation flow (L/min) Top-bottom split (K) Profile exit temp (°C)
100 (stagnant) 10.0 45
250 5.0 37
325 2.8 34
400 (specified) 1.2 32

Table 1 - Recirculation flow against stratification and exit temperature

Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.

Trace the warm layer to the flow design

In 27 commissioning audits the split traced to a stagnant top layer, an undersized chiller, blocked nozzles, a poor inlet header and a short tank. One dead leg can stratify the tank within 20 minutes of start-up.

A five-step diagnostic sequence

  1. Log three depths first.
    Measure water temperature at the surface, mid-depth and bottom after 20 minutes; a 10 K split is the fault, not the die.
  2. Check recirculation flow.
    Read the flowmeter at the header; 100 L/min instead of 400 L/min explains both the split and the 45 °C exit.
  3. Inspect nozzles and baffles.
    Find blocked spray rows and confirm baffle spacing of 1.5 m or less; one dead leg stratifies the tank quickly.
  4. Verify chiller capacity.
    Log inlet temperature through a full shift; an undersized chiller lets it climb from 14 °C to 22 °C.
  5. Run the flow trial.
    Step 100, 250, 325 and 400 L/min and log three depths; the 10.0 to 1.2 K fall proves the tank design.

The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

A 6 m cooling tank with a 10 K split from top to bottom: the profile is leaving too hot: measured data and the leading root causes
Figure 1 — Measured response and the distribution of root causes found in field audits.

Set the water parameters that quench evenly

Four settings give an even quench: a top-to-bottom difference under 3 K, water velocity of 0.25-0.4 m/s, an exit temperature of 30-35 °C, and baffles at 1.5 m spacing or less. Below 0.1 m/s a warm boundary layer clings to the profile.

المعلمة Typical target What goes wrong outside it
Top / bottom water difference, 6 m tank 3 K or less A 10 K split sets differential shrink and a permanent bow
Water velocity over the profile 0.25-0.4 m/s Below 0.1 m/s a warm boundary layer clings to the surface
Profile temperature at tank exit 30-35 °C Above 42 °C the part keeps shrinking after the saw
Baffle / header spacing 1.5 m or less Unbaffled tanks stratify within 20 minutes of start-up

Table 2 - Tank settings that quench a rigid PVC profile evenly

Prove it with a recirculation-flow trial

Run a recirculation-flow trial at fixed output: set 100, 250, 325 and 400 L/min and log three depths. The split falls 10.0, 5.0, 2.8 then 1.2 K while exit temperature drops 45 to 32 °C, clearing the 3 K limit at 325 L/min.

Field symptom Most likely cause Check that confirms it
Top water warm, bottom cold Stagnant layer, no baffles Three-depth log shows a 10 K split
Length scatter after start-up Profile leaving the tank hot Exit probe reads 45 °C instead of 32 °C
One face of the profile shinier Blocked spray nozzle row Nozzle pressure reads zero on that header
Split worsens through the shift Undersized chiller Inlet temperature climbs from 14 °C to 22 °C

Table 3 - Matching the tank symptom to the flow fault

Myth: "A process adjustment will fix it." Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.

Write the tank acceptance into the commissioning order

Write the tank acceptance into the commissioning order: a 3 K limit measured at three depths, minimum recirculation flow and exit temperature at rated output. One shared ramp turns a 10 K dispute into a flow figure, not a new die.

Need the section checked before tooling?

Send us the section and the installation conditions. We will review wall balance, tolerance and fixing detail, then return a marked-up drawing with a tooling quotation.

What to send us

  • Cross-section drawing with wall thicknesses
  • Material and colour
  • Installation temperature range
  • Fixing method and run length

Send the section drawing

What an even quench saves over a year

An even quench protects downstream length. At 2.4 m/min the line makes about 8 km a day; 400 L/min holds a 1.2 K split and 32 °C exit, while a blocked header adds ±6 mm of cut scatter before the saw is checked.

Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.

Before you release this extruded profile

  • A 3 K top-to-bottom limit measured at three depths is specified
  • Minimum recirculation flow in L/min appears in the commissioning order
  • Profile exit temperature at rated output is written into the sign-off
  • Baffle or header spacing of 1.5 m or less is required
  • Chiller capacity and inlet temperature are stated for a full shift

Write the measurement temperature and the tolerance into the drawing; most disputes are really about how the part was measured.

Why is my cooling tank 24 °C at the top and 14 °C at the bottom?

Warm water rises and an unbaffled tank has no mixing. At 100 L/min we logged a 10 K split; at 400 L/min with baffles it fell to 1.2 K.

Does the water temperature really affect the profile?

Yes. A 10 K split quenches the upper face more slowly, so the part leaves at 45 °C instead of 32 °C and keeps shrinking after the saw, adding about ±6 mm of cut-length scatter.

What top-to-bottom difference should I allow?

3 K or less. Above that the differential shrink can set a permanent bow. Measure at three depths after 20 minutes of running, not at the inlet alone.

How much recirculation flow does a 6 m tank need?

In our trial 325 L/min cleared the 3 K limit and 400 L/min held 1.2 K, with water velocity around 0.3 m/s over the profile. Below 0.1 m/s a warm boundary layer clings to the surface.

Will a bigger chiller fix stratification?

It helps the heat load but not the mixing. Blocked nozzles, a poor inlet header and missing baffles are the leading causes in 27 audits; fix the distribution first.

What should commissioning sign-off include?

A 3 K limit at three depths, minimum flow, exit temperature at rated output, baffle spacing and chiller capacity. Then a 10 K dispute is settled with a flowmeter reading.

Get a profile that holds its dimension

Send us the profile section, the length and the service conditions. We will review die, calibration and tolerance, then quote tooling and production with a defined measurement method.

To get an accurate quote, send:

  • Profile cross-section drawing
  • Material and colour
  • Cut length and annual volume
  • Service temperature and exposure

Request a profile quotation

أحدث المنشورات

واتساب
فيسبوك
تويتر
لينكد إن
بينتيريست
Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
arAR

اطلب عرض أسعار سريع

إرسال الرسومات والمتطلبات التفصيلية عبر

Emial: [email protected]

أو املأ نموذج الاتصال أدناه: