{"id":8767,"date":"2026-08-28T09:00:00","date_gmt":"2026-08-28T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/extrusion-surface-scratch\/"},"modified":"2026-11-02T02:25:59","modified_gmt":"2026-11-02T02:25:59","slug":"extrusion-surface-scratch","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ru\/extrusion-surface-scratch\/","title":{"rendered":"Surface Scratches: From the Sizing Sleeve to the Packing Table"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/extrusion-surface-scratch.jpg\" alt=\"The haul-off unit of an extrusion line gripping a white PVC profile between two rubber belts with a scuff visible behind the belt\" width=\"1536\" height=\"909\"><figcaption>Every metre of profile passes this point, and the belt is the usual suspect.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"distinguish\">A scratch is not a die line<\/h2>\n<p>The first distinction is between a mark made by the die and a mark made after it. A die line is a copy of an irregularity on the die land: it is continuous for the whole run, it has a fixed position on the face, and it does not change with line speed. A scratch is a contact mark: it is usually intermittent, it can change position, and it is often visible only on part of the length.<\/p>\n<p>The second distinction is between a scratch and a handling mark. A scratch has a direction and a depth; a handling mark is a scuff with no clear direction. Scratches come from something moving relative to the profile at speed, which means the line. Scuffs come from the profile moving against something at low speed, which means packing and transport.<\/p>\n<p>The third is between a mark in the surface and a mark through it. A shallow scratch on a glossy white profile is a cosmetic defect. A scratch deep enough to break the surface of a capped or co-extruded profile exposes the substrate and becomes a weathering and colour problem, which is a different severity and a different conversation.<\/p>\n<p>Getting these three distinctions right at the start saves the most common wasted effort in this area, which is polishing a die that was never the cause. A die that produces a clean surface at low speed and a scratched one at production speed is telling you the mark is downstream.<\/p>\n<h2 id=\"belt\">Belt pressure has a threshold, not a trend<\/h2>\n<p>The chart on the left plots coil rejection against haul-off belt pressure. At 0.8 bar rejection is 1.2 percent, at 1.5 bar 2.0, at 2.5 bar 5.0, at 3.5 bar 11.0 and at 4.5 bar 19.0. The shaded zone from 2.5 bar upward is where scratches dominate the reject list.<\/p>\n<figure>\n<img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/extrusion-surface-scratch-chart.jpg\" alt=\"Coil rejection against haul-off belt pressure with a scratch zone marked, and a bar chart of where scratches are traced to\" width=\"1536\" height=\"909\"><figcaption>Left: rejection climbs steeply past 2.5 bar. Right: the sleeve entry and the belt account for half of all scratches.<\/figcaption><\/figure>\n<p>The important feature is that the curve is not smooth. Between 0.8 and 1.5 bar the increase is small, and it is mostly the normal consequence of gripping harder. Past 2.5 bar it turns up sharply, because the belt has started to slip and recover rather than grip continuously, and every slip is a rub.<\/p>\n<p>That is why the fix is not always to reduce pressure. A belt that is too loose also slips, and a slipping belt scratches more than a tight one. The target is the lowest pressure at which the belt does not slip, which is found by testing at the lowest setting and increasing until the profile stops wandering.<\/p>\n<p>Belt condition matters as much as pressure. A belt with compound embedded in it, or with a hardened, glazed surface, scratches at any pressure. Belts are consumables and should be replaced on condition, not on failure, and the condition to look for is a shiny surface and embedded white residue.<\/p>\n<h2 id=\"sources\">The six contact points, in order<\/h2>\n<p>The right hand panel gives the distribution: sizing sleeve entry 28 percent, haul-off belt 24, cooling conveyor roller 18, saw infeed 14, packing table 10. Together the first two are more than half, which is where the inspection should start.<\/p>\n<p>The sizing sleeve entry is the highest because it is where the profile is hottest and softest and where the clearance is smallest. A burr on the entry radius, a chip in the sleeve, or a piece of flash caught between the profile and the sleeve will mark every metre. The mark from a sleeve entry is continuous and has a fixed position, which distinguishes it from a belt mark.<\/p>\n<p>The cooling conveyor roller is third because the profile is still warm when it passes over it. A roller that has stopped turning, or one with a flat spot, rubs rather than rolls. The mark is periodic, with a spacing equal to the roller circumference, which is a diagnosis in itself.<\/p>\n<p>The saw infeed and the packing table are the low-speed contacts, and they produce scuffs rather than scratches. They matter on a glossy profile and they matter more in summer, when the profile is softer when it reaches the saw.<\/p>\n<h2 id=\"trace\">Tracing a scratch in twenty minutes<\/h2>\n<p>The method is to stop the line with a length of scratched profile still on it, and look at where the mark begins and ends. A mark that exists at the tank exit but not at the die has a cause between them. A mark that appears only after the haul-off has a cause downstream. This single observation usually halves the search.<\/p>\n<p>The second step is to mark the profile with a felt pen at the position of the scratch and run it slowly by hand through each unit in turn. A scratch that appears after a specific unit has found its cause. It takes twenty minutes and it is far more reliable than reasoning about which unit is most likely.<\/p>\n<p>The third step is to check the position around the section. A scratch on the top face comes from something above; a scratch on a corner comes from a guide or a roller edge; a scratch on the inside of a hollow profile comes from a calibration mandrel or an internal air plug, which is a different set of causes entirely.<\/p>\n<table>\n<thead>\n<tr>\n<th>Mark pattern<\/th>\n<th>Likely source<\/th>\n<th>Check<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Continuous, fixed position<\/td>\n<td>Sizing sleeve entry or die land<\/td>\n<td>Entry radius, sleeve bore, flash<\/td>\n<\/tr>\n<tr>\n<td>Periodic, regular spacing<\/td>\n<td>A roller with a flat or a stopped rotation<\/td>\n<td>Roller freedom, circumference against spacing<\/td>\n<\/tr>\n<tr>\n<td>Intermittent, one face<\/td>\n<td>Haul-off belt slip<\/td>\n<td>Belt pressure, belt condition<\/td>\n<\/tr>\n<tr>\n<td>At the cut end only<\/td>\n<td>Saw infeed guide<\/td>\n<td>Guide clearance, swarf<\/td>\n<\/tr>\n<tr>\n<td>All over, dull<\/td>\n<td>Packing and transport<\/td>\n<td>Stillage surface, strapping<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 Reading the pattern of a mark to find the unit responsible.<\/p>\n<h2 id=\"prevent\">Prevention is cheaper than detection<\/h2>\n<p>The prevention list is short. Guides and rollers should be a material that is softer than the profile and should be free to rotate. Contact points should be the minimum number needed to control the profile, because every additional contact is an additional scratch risk. And the line should be laid out so that the profile is not dragged over anything between units.<\/p>\n<p>The second item is cleanliness. A scratch is often caused by a particle: a chip of PVC, a piece of grit, a hardened drip of compound. A wipe-down of the contact points at every start-up is a two minute job that removes a fault class, and it is the first thing to be dropped when the line is busy.<\/p>\n<p>The third is the packing specification. A profile stacked on a bare stillage, or strapped directly against a steel edge, will be marked in transit no matter how good the line is. A liner, a soft strap and a limit on stack height are cheap, and they are the difference between a claim and no claim.<\/p>\n<p>The fourth is the record. A shop that knows which unit caused the last three scratch complaints can prioritise maintenance. A shop that treats each complaint as new will keep polishing the die and keep receiving the same complaint.<\/p>\n<table>\n<thead>\n<tr>\n<th>Contact point<\/th>\n<th>What to check<\/th>\n<th>Interval<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Sizing sleeve entry<\/td>\n<td>Radius, burrs, flash trapped at the entry<\/td>\n<td>Every start-up<\/td>\n<\/tr>\n<tr>\n<td>Haul-off belt<\/td>\n<td>Pressure, glazing, embedded compound<\/td>\n<td>Every shift<\/td>\n<\/tr>\n<tr>\n<td>Cooling conveyor rollers<\/td>\n<td>Free rotation, flat spots, build-up<\/td>\n<td>Weekly<\/td>\n<\/tr>\n<tr>\n<td>Saw infeed guides<\/td>\n<td>Clearance, swarf, guide material<\/td>\n<td>Every shift<\/td>\n<\/tr>\n<tr>\n<td>Packing stillage<\/td>\n<td>Liner present, strap edges padded<\/td>\n<td>Every stack<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 A contact point checklist, cheapest fix first.<\/p>\n<h2 id=\"cost\">What a scratch actually costs<\/h2>\n<p>The direct cost is the rejected length, and on a continuous profile that is usually small. The indirect cost is larger: a customer who finds scratches inspects more, and an inspecting customer finds everything else as well. The relationship damage from a recurring cosmetic defect is out of proportion to the defect.<\/p>\n<p>There is also a sorting cost that is easy to underestimate. A coil with an intermittent scratch cannot be scrapped as a whole if most of it is good, so it is unwound, inspected and re-coiled, which is manual work at a rate far above the cost of making it in the first place.<\/p>\n<p>Which is why the threshold in the belt curve matters commercially. Going from 3.5 bar to 2.5 bar on a line that is rejecting 11 percent of coils for scratches is worth more than the throughput lost by running a slightly looser belt. The trade is not close.<\/p>\n<div class=\"faq\">\n<h3>How do I tell a scratch from a die line?<\/h3>\n<p>A die line is continuous for the whole run, has a fixed position on the face and does not change with line speed. A scratch is usually intermittent, can change position, and often appears only on part of the length. The speed test separates them quickly.<\/p>\n<h3>What causes scratches on an extruded profile?<\/h3>\n<p>Contact at speed. The sizing sleeve entry and the haul-off belt account for about half of all cases, followed by cooling conveyor rollers, the saw infeed and the packing table.<\/p>\n<h3>Is lower haul-off belt pressure always better?<\/h3>\n<p>No. A belt that is too loose slips, and a slipping belt scratches more than a tight one. The target is the lowest pressure at which the belt does not slip, found by starting low and increasing until the profile stops wandering.<\/p>\n<h3>Why is the rejection rate so sensitive to belt pressure?<\/h3>\n<p>Because past about 2.5 bar the belt starts to slip and recover rather than grip continuously, and every slip is a rub. The curve is a threshold rather than a straight line for that reason.<\/p>\n<h3>How do I trace a scratch to a specific machine?<\/h3>\n<p>Stop the line with the scratched length still on it, note where the mark begins and ends, then run the profile slowly by hand through each unit in turn with a felt pen mark at the scratch position. The unit where the mark appears is the cause.<\/p>\n<h3>Why do scratches appear only on one face?<\/h3>\n<p>Because the cause is on that side. A guide, a roller edge or a belt on one side of the line will mark only the face it touches. A mark on the inside of a hollow profile points at a calibration mandrel or an internal air plug.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">A surface that arrives clean<\/p>\n<p>Send us the profile, the surface finish and a photograph of the mark. We will tell you which contact point the pattern points to, and what the line has to change to stop making it.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ru\/%d0%bf%d0%b2%d1%85-%d0%bf%d1%80%d0%be%d1%84%d0%b8%d0%bb%d0%b8\/\">Discuss a surface defect<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ru\/extrusion-die-lines\/\">Die Lines: Tracing a Longitudinal Mark<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ru\/extrusion-haul-off-speed\/\">Haul-Off Speed and What It Controls<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ru\/extrusion-vacuum-sizing\/\">Vacuum Sizing: What a Calibrator Actually Does<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ru\/extrusion-water-bath-cooling\/\">Extrusion Water Bath Cooling: Length and Temperature<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ru\/profile-packaging-handling\/\">Profile Packaging and Handling<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>A scratch is a contact mark, and the profile touches six things between the die and the pallet. Finding which one is a matter of following the line, not of polishing the die again.<\/p>","protected":false},"author":1,"featured_media":8765,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[17],"tags":[],"class_list":["post-8767","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-plastic-extrusion-process"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/posts\/8767","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/comments?post=8767"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/posts\/8767\/revisions"}],"predecessor-version":[{"id":8831,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/posts\/8767\/revisions\/8831"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/media\/8765"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/media?parent=8767"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/categories?post=8767"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/tags?post=8767"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}