{"id":7731,"date":"2025-09-06T09:00:00","date_gmt":"2025-09-06T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/laser-cutting-acrylic\/"},"modified":"2026-10-28T03:47:24","modified_gmt":"2026-10-28T03:47:24","slug":"laser-cutting-acrylic","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ru\/laser-cutting-acrylic\/","title":{"rendered":"Laser Cutting Acrylic: Parameters, Edge Quality and Design Rules"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u81ea\u52a8\u5c55\u5f00\u7684\u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/laser-cutting-acrylic.jpg\" alt=\"CO2 laser cutting a clear acrylic sheet on a flatbed cutter with extraction running\" width=\"1536\" height=\"909\"><figcaption>A CO2 laser is the only common cutting process that leaves acrylic with a polished edge straight off the machine. Everything else about it is a compromise.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"intro\">The edge is the reason to use a laser<\/h2>\n<p>Acrylic can be cut with a saw, a router, a waterjet, a knife or a laser, and the machine choice usually gets made on tolerance or on price. That is the wrong order. The first question is what the cut edge has to look like, because only one of those processes produces an edge that does not need finishing.<\/p>\n<p>A saw leaves tooth marks and a crazed edge that must be jointed and polished. A router leaves a matte, machined surface that has to be flame-polished or buffed, and polishing is a skilled hand operation that costs more than the cutting. A laser leaves a glossy, transparent edge that looks as though it was polished at the factory, because in effect it was: the beam does not cut acrylic so much as depolymerise it, and the resolidified wall is smooth.<\/p>\n<p>That single property is why laser cutting dominates display work, signage, point-of-sale and anything where the edge is on show. It is also why the process is worth understanding: the polished edge is not free, and it degrades the moment the parameters drift.<\/p>\n<div class=\"callout\">\n<p><strong>The trade is edge quality against everything else.<\/strong> A laser gives you the best-looking edge and the worst dimensional stability of any cutting method, because it puts heat into a material with a thermal expansion coefficient of 70 \u00d7 10\u207b\u2076 per \u00b0C. Design around that and the process is excellent.<\/p>\n<\/div>\n<h2 id=\"mechanism\">What a CO2 laser actually does to PMMA<\/h2>\n<p>The beam wavelength is 10.6 \u00b5m, in the far infrared, and poly(methyl methacrylate) absorbs it almost completely within a few micrometres of the surface. There is no transmission through the sheet and no reflection worth worrying about. All the energy lands in a very thin layer.<\/p>\n<p>That layer does not melt and flow the way it would under a hot wire. PMMA is unusual among thermoplastics in that heating it far above its glass transition makes it unzip back into methyl methacrylate monomer rather than forming a viscous melt. The cut is a depolymerisation front: monomer vaporises, the pressure of the vapour clears the kerf, and the walls left behind are smooth and glassy.<\/p>\n<p>Two practical consequences follow. The edge is glossy without any secondary operation. And the vapour is methyl methacrylate, which has a distinct sweet smell that parts cut without extraction carry for days. Acrylic is also genuinely combustible in the beam: a small flame at the kerf is normal and is part of how the cut progresses, but a flame that persists after the beam has moved on is a fire, and it happens most often when the assist air is off or the sheet is masked with paper.<\/p>\n<h2 id=\"parameters\">Power, speed and the parameter window<\/h2>\n<p>Every machine has its own numbers, so treat the figures below as a starting window rather than a recipe. What matters is the shape of the relationship: as thickness rises, power rises and speed falls faster than linearly, because the beam has to remove a growing volume of material through a kerf that is getting deeper and narrower.<\/p>\n<table>\n<thead>\n<tr>\n<th>Cast acrylic thickness<\/th>\n<th>Beam power<\/th>\n<th>Cut speed<\/th>\n<th>Typical kerf<\/th>\n<th>Edge result<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>2 mm<\/td>\n<td>40 \u2013 60 W<\/td>\n<td>25 \u2013 40 mm\/s<\/td>\n<td>0.10 \u2013 0.15 mm<\/td>\n<td>Polished, near-vertical<\/td>\n<\/tr>\n<tr>\n<td>3 mm<\/td>\n<td>60 \u2013 80 W<\/td>\n<td>12 \u2013 18 mm\/s<\/td>\n<td>0.15 mm<\/td>\n<td>Polished, near-vertical<\/td>\n<\/tr>\n<tr>\n<td>5 mm<\/td>\n<td>80 \u2013 100 W<\/td>\n<td>8 \u2013 12 mm\/s<\/td>\n<td>0.15 \u2013 0.20 mm<\/td>\n<td>Polished, slight taper<\/td>\n<\/tr>\n<tr>\n<td>10 mm<\/td>\n<td>120 \u2013 140 W<\/td>\n<td>3 \u2013 5 mm\/s<\/td>\n<td>0.20 \u2013 0.25 mm<\/td>\n<td>Polished, visible striations<\/td>\n<\/tr>\n<tr>\n<td>15 mm<\/td>\n<td>140 \u2013 150 W<\/td>\n<td>1.5 \u2013 2.5 mm\/s<\/td>\n<td>0.25 \u2013 0.30 mm<\/td>\n<td>Polished, pronounced taper<\/td>\n<\/tr>\n<tr>\n<td>20 mm<\/td>\n<td>150 W+<\/td>\n<td>0.8 \u2013 1.2 mm\/s<\/td>\n<td>0.30 mm<\/td>\n<td>Glossy but wavy, needs finishing<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 Starting parameters for cast acrylic on a 100\u2013150 W CO2 flatbed. Speed falls by roughly a factor of thirty between 2 mm and 20 mm.<\/p>\n<p>The assist gas is where most operators get the edge wrong. Acrylic is normally cut with compressed air at very low pressure, around 0.2 to 0.5 bar, just enough to keep the lens clean and push the vapour out of the kerf. Raising the pressure to the 2 to 4 bar used on steel does clear the kerf better and does allow higher speed, but it also chills the wall before it can smooth itself, and the edge comes out frosted white instead of clear. Nitrogen gives the cleanest cut on thick material and a reliably matte edge \u2014 the right choice when the edge will be bonded and appearance does not matter, the wrong choice when the polished edge is the reason the job came to a laser.<\/p>\n<table>\n<thead>\n<tr>\n<th>Assist gas<\/th>\n<th>\u0414\u0430\u0432\u043b\u0435\u043d\u0438\u0435<\/th>\n<th>Edge appearance<\/th>\n<th>When to use<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Compressed air, low<\/td>\n<td>0.2 \u2013 0.5 bar<\/td>\n<td>Clear, glossy, flame-polished<\/td>\n<td>Default for display and visible edges<\/td>\n<\/tr>\n<tr>\n<td>Compressed air, high<\/td>\n<td>2 \u2013 4 bar<\/td>\n<td>Frosted white<\/td>\n<td>Speed-critical work on hidden edges<\/td>\n<\/tr>\n<tr>\n<td>Nitrogen<\/td>\n<td>4 \u2013 8 bar<\/td>\n<td>Matte, uniform, no oxidation<\/td>\n<td>Thick sections, parts to be bonded<\/td>\n<\/tr>\n<tr>\n<td>None<\/td>\n<td>\u2014<\/td>\n<td>Glossy but smoky, soot deposits<\/td>\n<td>Not recommended \u2014 fire and lens risk<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 Assist gas. The difference between a clear edge and a white one is usually the regulator, not the machine.<\/p>\n<p>Focus position is the other lever. Focusing on the top surface gives the narrowest kerf and the fastest cut on thin sheet. Focusing a millimetre or two below the surface on 10 mm and above produces a more parallel wall, because the beam waist sits in the middle of the thickness and the natural V-shape of the kerf is partly cancelled.<\/p>\n<h2 id=\"cast-vs-extruded\">Cast and extruded do not cut the same<\/h2>\n<p>This is the single most common source of complaint, and it is almost never the machine's fault. Cast and extruded acrylic are chemically the same polymer but differ in molecular weight and in residual stress, and the beam exposes both differences.<\/p>\n<table>\n<thead>\n<tr>\n<th>Behaviour under the beam<\/th>\n<th>Cast acrylic<\/th>\n<th>Extruded acrylic<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Edge after cutting<\/td>\n<td>Glossy, water-clear<\/td>\n<td>Glossy but often faintly hazy<\/td>\n<\/tr>\n<tr>\n<td>Bubbles or trails in the edge<\/td>\n<td>Rare<\/td>\n<td>Common, especially above 6 mm<\/td>\n<\/tr>\n<tr>\n<td>Cutting speed<\/td>\n<td>\u041c\u0435\u0434\u043b\u0435\u043d\u043d\u0435\u0435<\/td>\n<td>\u0411\u044b\u0441\u0442\u0440\u0435\u0435<\/td>\n<\/tr>\n<tr>\n<td>Kerf consistency<\/td>\n<td>Stable<\/td>\n<td>More variation sheet to sheet<\/td>\n<\/tr>\n<tr>\n<td>Crazing after solvent bonding<\/td>\n<td>Low risk<\/td>\n<td>Higher risk<\/td>\n<\/tr>\n<tr>\n<td>Maximum clean thickness<\/td>\n<td>25 mm and beyond<\/td>\n<td>Around 10 \u2013 12 mm<\/td>\n<\/tr>\n<tr>\n<td>Sheet flatness after cutting<\/td>\n<td>\u0425\u043e\u0440\u043e\u0448\u043e<\/td>\n<td>Can bow as stress releases<\/td>\n<\/tr>\n<tr>\n<td>Relative cost<\/td>\n<td>\u0412\u044b\u0448\u0435<\/td>\n<td>\u041d\u0438\u0436\u043d\u0438\u0439<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 \u2014 Cast versus extruded under a CO2 beam. The bubble trails in extruded material are volatiles released from a lower-molecular-weight resin, not a parameter error.<\/p>\n<p>Extruded sheet is made continuously and cooled fast, which locks in oriented stress and leaves more residual monomer and moisture. Under the beam, that volatiles burst out through the resolidifying wall and leave the fine bubble trails that show up as a milky streak along the edge. No amount of parameter tuning removes them entirely; the material is telling you what it is. Cast sheet is cell-cast or continuously cast and then annealed, so it is more relaxed and cleaner. It cuts slower because the higher molecular weight takes more energy to unzip, but the edge is the one people picture when they say \"laser-cut acrylic\".<\/p>\n<div class=\"callout\">\n<p><strong>If the edge will be visible, specify cast.<\/strong> If the part is a sign backer or an internal bracket where nobody looks at the edge, extruded cuts faster and costs less. Mixing the two on one drawing is how a batch ends up with half the parts looking different.<\/p>\n<\/div>\n<h2 id=\"thickness\">How thick can you go<\/h2>\n<p>Sales literature quotes 25 mm and sometimes 30 mm. Production reality is different, because the question is not whether the beam gets through but whether the edge is still acceptable at the bottom.<\/p>\n<p>The limit is set by the aspect ratio of the kerf. As thickness rises, the kerf narrows relative to its depth, the vapour has further to travel to escape, and it deposits heat on the walls on the way out. The result is striations \u2014 the vertical ripple pattern on the cut face \u2014 and a taper where the top of the cut is wider than the bottom. Neither is a failed cut, but both are visible on a clear edge.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0422\u043e\u043b\u0449\u0438\u043d\u0430<\/th>\n<th>Single pass<\/th>\n<th>Edge quality<\/th>\n<th>Practical note<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1 \u2013 5 mm<\/td>\n<td>\u0414\u0430<\/td>\n<td>\u041f\u0440\u0435\u0432\u043e\u0441\u0445\u043e\u0434\u043d\u043e<\/td>\n<td>No secondary operation needed<\/td>\n<\/tr>\n<tr>\n<td>5 \u2013 10 mm<\/td>\n<td>\u0414\u0430<\/td>\n<td>\u0425\u043e\u0440\u043e\u0448\u043e<\/td>\n<td>Focus below surface; taper measurable<\/td>\n<\/tr>\n<tr>\n<td>10 \u2013 15 mm<\/td>\n<td>\u0414\u0430<\/td>\n<td>Acceptable<\/td>\n<td>Striations visible under raking light<\/td>\n<\/tr>\n<tr>\n<td>15 \u2013 20 mm<\/td>\n<td>Yes, slow<\/td>\n<td>\u042f\u0440\u043c\u0430\u0440\u043a\u0430<\/td>\n<td>Edge often needs a light polish for display<\/td>\n<\/tr>\n<tr>\n<td>20 \u2013 25 mm<\/td>\n<td>Marginal<\/td>\n<td>\u0411\u0435\u0434\u043d\u044b\u0439<\/td>\n<td>Consider sawing and machining instead<\/td>\n<\/tr>\n<tr>\n<td>Over 25 mm<\/td>\n<td>\u041d\u0435\u0442<\/td>\n<td>\u2014<\/td>\n<td>Route or saw, then polish<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 4 \u2014 Thickness capability. Multiple passes are not a solution on acrylic: the second pass re-melts the first and doubles the striation pattern.<\/p>\n<p>Multiple passes are widely assumed to solve thick material and they do not. On metal, a second pass can deepen a kerf usefully. On acrylic, the first pass has already left a glossy wall; the second pass runs down that wall, re-heats it, and leaves a stepped, rippled surface that looks worse than a single slow pass.<\/p>\n<h2 id=\"defects\">The defects and what actually causes them<\/h2>\n<p>Almost every laser cutting complaint resolves to one of eight causes, and most of them are visible in the first ten seconds of looking at the part.<\/p>\n<table>\n<thead>\n<tr>\n<th>Symptom<\/th>\n<th>\u041f\u0440\u0438\u0447\u0438\u043d\u0430<\/th>\n<th>Fix<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Frosted white edge<\/td>\n<td>Assist pressure too high, or power too high for the speed<\/td>\n<td>Drop air to 0.3 bar, raise speed<\/td>\n<\/tr>\n<tr>\n<td>Brown or scorched edge<\/td>\n<td>Speed too slow for the power, dirty lens, defocused beam<\/td>\n<td>Clean optics, re-focus, increase speed<\/td>\n<\/tr>\n<tr>\n<td>Vertical striations<\/td>\n<td>Speed too high, focal point above the surface<\/td>\n<td>Slow down 20%, focus into the material<\/td>\n<\/tr>\n<tr>\n<td>Dross or beads on the underside<\/td>\n<td>Speed too slow, focus too high, insufficient assist<\/td>\n<td>Increase speed, lower focus, add air<\/td>\n<\/tr>\n<tr>\n<td>Bubble trails in the edge<\/td>\n<td>Extruded sheet, or damp material<\/td>\n<td>Switch to cast, store sheet dry<\/td>\n<\/tr>\n<tr>\n<td>Visible taper<\/td>\n<td>Short focal length lens, focus at surface<\/td>\n<td>Longer focal lens, focus below surface<\/td>\n<\/tr>\n<tr>\n<td>Crazing after solvent bonding<\/td>\n<td>Heat-affected zone left stressed, solvent attack<\/td>\n<td>Anneal before bonding<\/td>\n<\/tr>\n<tr>\n<td>Flame that persists<\/td>\n<td>No assist gas, paper masking, slow corner moves<\/td>\n<td>Restore air, remove paper mask, tune corners<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 5 \u2014 Defect diagnosis. The heat-affected zone is only 0.1\u20130.3 mm deep, but it is where every bonding failure starts.<\/p>\n<p>The heat-affected zone deserves more attention than it gets. It is thin \u2014 typically 0.1 to 0.3 mm \u2014 but within it the polymer has been through a violent thermal cycle and carries locked-in stress and a small population of micro-cracks. The edge looks perfect and behaves badly. Solvent applied to that edge wicks into the micro-cracks, softens the stressed layer, and the crack propagates. The part crazes along the bond line two hours after assembly and the adhesive gets blamed.<\/p>\n<p>Annealing fixes it. For acrylic, the standard cycle is roughly one hour at 80 \u00b0C per 3 mm of thickness, followed by cooling no faster than 10 \u00b0C per hour, so a 5 mm part needs about two hours at temperature plus a slow ramp down. It is an unglamorous step that adds a day to the schedule and is the difference between a bonded assembly that survives a drop test and one that does not.<\/p>\n<h2 id=\"tolerances\">Tolerances: what the machine holds and what the material takes back<\/h2>\n<p>Laser positioning accuracy is impressive and largely irrelevant. The gantry will put the head within \u00b10.05 mm of where it was told. The part will not be within \u00b10.05 mm of the drawing, because the material moves.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0425\u0430\u0440\u0430\u043a\u0442\u0435\u0440\u0438\u0441\u0442\u0438\u043a\u0430<\/th>\n<th>Machine capability<\/th>\n<th>Realistic part tolerance<\/th>\n<th>Limiting factor<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Position of a cut feature<\/td>\n<td>\u00b10.05 mm<\/td>\n<td>\u00b10.10 mm<\/td>\n<td>Kerf variation<\/td>\n<\/tr>\n<tr>\n<td>Edge-to-edge distance<\/td>\n<td>\u00b10.05 mm<\/td>\n<td>\u00b10.15 mm<\/td>\n<td>Kerf variation, taper<\/td>\n<\/tr>\n<tr>\n<td>Hole diameter, under 10 mm<\/td>\n<td>\u00b10.08 mm<\/td>\n<td>\u00b10.15 mm<\/td>\n<td>Hole comes out slightly tapered<\/td>\n<\/tr>\n<tr>\n<td>Part length, 1 m<\/td>\n<td>\u00b10.05 mm<\/td>\n<td>\u00b10.30 mm<\/td>\n<td>Thermal expansion of the sheet<\/td>\n<\/tr>\n<tr>\n<td>Part length, 2 m<\/td>\n<td>\u00b10.05 mm<\/td>\n<td>\u00b10.60 mm<\/td>\n<td>Thermal expansion, sheet bow<\/td>\n<\/tr>\n<tr>\n<td>Flatness<\/td>\n<td>Not controlled<\/td>\n<td>1 \u2013 3 mm per metre<\/td>\n<td>Stress relief in the sheet<\/td>\n<\/tr>\n<tr>\n<td>Edge squareness<\/td>\n<td>\u2014<\/td>\n<td>0.1 \u2013 0.3 mm over 10 mm<\/td>\n<td>Beam taper<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 6 \u2014 Tolerance capability. Above about 500 mm, thermal expansion of the material dominates everything the machine does.<\/p>\n<p>The thermal expansion number is worth internalising. Acrylic expands by about 70 \u00d7 10\u207b\u2076 per \u00b0C, roughly seven times steel and twenty times glass. A one-metre part measured at 15 \u00b0C in the morning and at 25 \u00b0C in the afternoon is 0.7 mm longer in the afternoon. If the drawing calls for \u00b10.2 mm over a metre, the part cannot comply in a workshop without temperature control, no matter which machine cut it.<\/p>\n<p>Flatness is the other trap. Laser cutting does not bend the sheet, but releasing the internal stress of a sheet by cutting a large shape out of it does. A panel that was flat on the bed can bow 2 or 3 mm across a metre by the time it is off the machine, and no tolerance on the drawing will change that.<\/p>\n<h2 id=\"design\">Design rules for the drawing<\/h2>\n<p>Laser cutting removes material along a path of finite width, so the drawing has to account for the kerf. Every profile is offset outward by half the kerf width \u2014 0.075 mm for a 0.15 mm kerf \u2014 and the nesting software normally does this automatically. What the software cannot fix is geometry that is too small to cut.<\/p>\n<ul>\n<li><strong>Minimum hole diameter<\/strong> \u2014 about 0.8 times the material thickness, and one times the thickness for a hole that must be round and clean. A 2 mm hole in 10 mm acrylic will come out tapered and slightly oval.<\/li>\n<li><strong>Minimum web between features<\/strong> \u2014 one times the thickness. Thinner webs overheat, distort and sometimes collapse.<\/li>\n<li><strong>Minimum slot width<\/strong> \u2014 0.8 times the thickness, and no slot longer than about ten times its width without a bridge.<\/li>\n<li><strong>Corner radius<\/strong> \u2014 0.5 mm minimum on internal corners. The beam can turn a sharp corner, but the corner concentrates stress and becomes the crack origin in service.<\/li>\n<li><strong>Nesting gap<\/strong> \u2014 3 mm minimum between parts. Closer than that and the heat from one cut affects the neighbour's edge.<\/li>\n<li><strong>Lead-in<\/strong> \u2014 on material over 8 mm, start the cut on a scrap tab or outside the profile and run in, otherwise the pierce leaves a dimple on the finished edge.<\/li>\n<li><strong>Tabs<\/strong> \u2014 small parts need uncut tabs or they drop through the bed and jam the machine.<\/li>\n<\/ul>\n<p>The kerf also has to be declared if the part fits into something else. A panel cut to 500.00 mm nominal is actually 500.15 mm across the outside if the kerf was not compensated, and it will not fit a 500 mm frame. This is why a first article should always be measured rather than assumed.<\/p>\n<h2 id=\"versus\">When not to use a laser<\/h2>\n<p>Laser cutting is not the right answer for every acrylic part, and knowing where it stops saves a lot of expensive rework.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0420\u0430\u0441\u0441\u043c\u043e\u0442\u0440\u0435\u043d\u0438\u0435<\/th>\n<th>CO2 laser<\/th>\n<th>CNC router<\/th>\n<th>Panel saw<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Edge as cut<\/td>\n<td>Polished, clear<\/td>\n<td>Matte, needs polishing<\/td>\n<td>Saw marks, needs jointing<\/td>\n<\/tr>\n<tr>\n<td>Cutting force on the part<\/td>\n<td>None<\/td>\n<td>High, needs clamping<\/td>\n<td>\u0412\u044b\u0441\u043e\u043a\u0438\u0439<\/td>\n<\/tr>\n<tr>\n<td>Smallest internal feature<\/td>\n<td>0.5 mm<\/td>\n<td>Tool diameter, typically 3 mm<\/td>\n<td>None \u2014 straight cuts only<\/td>\n<\/tr>\n<tr>\n<td>Maximum thickness<\/td>\n<td>20 mm practical<\/td>\n<td>50 mm and beyond<\/td>\n<td>30 mm<\/td>\n<\/tr>\n<tr>\n<td>Speed on 3 mm sheet<\/td>\n<td>\u0411\u044b\u0441\u0442\u0440\u044b\u0439<\/td>\n<td>\u041c\u0435\u0434\u043b\u0435\u043d\u043d\u0435\u0435<\/td>\n<td>Fastest, straight only<\/td>\n<\/tr>\n<tr>\n<td>Heat input<\/td>\n<td>HAZ 0.1 \u2013 0.3 mm<\/td>\n<td>None<\/td>\n<td>None<\/td>\n<\/tr>\n<tr>\n<td>Typical tolerance<\/td>\n<td>\u00b10.15 mm<\/td>\n<td>\u00b10.10 mm<\/td>\n<td>\u00b10.30 mm<\/td>\n<\/tr>\n<tr>\n<td>Edge finish operation<\/td>\n<td>None<\/td>\n<td>Flame polish or buff<\/td>\n<td>Joint and polish<\/td>\n<\/tr>\n<tr>\n<td>Setup cost<\/td>\n<td>\u041d\u0438\u0437\u043a\u0438\u0439<\/td>\n<td>Medium, fixturing<\/td>\n<td>Very low<\/td>\n<\/tr>\n<tr>\n<td>\u041b\u0443\u0447\u0448\u0435\u0435 \u0434\u043b\u044f<\/td>\n<td>Thin to medium sheet, shaped cutouts<\/td>\n<td>Thick sheet, 3D machining, tight tolerance<\/td>\n<td>Straight cuts, high volume<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 7 \u2014 Process comparison. The router wins on thickness and tolerance; the laser wins on edge finish and on anything with a shaped internal cutout.<\/p>\n<p>Two material cases deserve a warning. Polycarbonate laser-cuts badly: it does not depolymerise cleanly, so the edge comes out amber to brown, it flames more readily than acrylic, and the cut edge is weaker than the base material. A laser is not the way to cut a polycarbonate guard. And PVC sheet must never go into a laser at all \u2014 it releases hydrogen chloride, which attacks the optics, the lens and every steel surface in the machine. One PVC job can write off a lens and corrode a gantry.<\/p>\n<div class=\"myth\">\n<p><b>Common assumption:<\/b> \"It is a laser, so it will cut anything plastic.\"<\/p>\n<p>It will cut acrylic beautifully and polycarbonate badly, and it will damage itself on anything chlorinated. Acrylic, PETG and most styrenics are fine. PVC, polyurethane foam and any flame-retardant grade containing halogens are not.<\/p>\n<\/div>\n<h2 id=\"safety\">Extraction, fire and the smell<\/h2>\n<p>The vapour from cutting acrylic is methyl methacrylate monomer, and it is not a nuisance odour to be tolerated. It is a respiratory irritant, and at the concentrations produced in a production cut it needs to be captured at the kerf and exhausted outside, not filtered and recirculated into the workshop. Extraction also protects the cut quality: vapour left hanging over the kerf deposits a fine white film on the surrounding sheet and on the lens, and a dirty lens absorbs energy, defocuses, and produces the brown edge that then gets blamed on the parameters.<\/p>\n<p>Fire is the real risk. Acrylic burns vigorously once alight, and a laser cutter is a machine that deliberately concentrates heat inside a combustible material. Never leave the machine running unattended, keep a clean bed with no offcuts under the workpiece, and remove paper masking before cutting. Paper masking in particular will smoulder and then ignite, and it is the most common cause of small fires in acrylic cutting.<\/p>\n<div class=\"faq\">\n<h3>Why is my laser-cut acrylic edge white instead of clear?<\/h3>\n<p>Almost always assist gas pressure. Air at 2 bar or more cools the kerf wall before it can smooth, leaving a frosted surface. Drop to 0.3\u20130.5 bar, keep the lens clean, and the edge comes back clear. If it does not, the power is too high for the speed.<\/p>\n<h3>Can a laser cut 20 mm acrylic?<\/h3>\n<p>Yes, on a 150 W machine at around 1 mm\/s, but the edge will be glossy with visible striations and a measurable taper. If the edge is on show, saw it and machine it instead. Twenty millimetres is the practical ceiling for a good-looking laser edge.<\/p>\n<h3>What kerf should I allow in the drawing?<\/h3>\n<p>0.15 mm for 2\u20135 mm sheet, 0.20 mm for 5\u201310 mm, and 0.25\u20130.30 mm above that. Offset the profile by half the kerf on each side. Most nesting software does this automatically, but the value has to be measured on the actual machine and material.<\/p>\n<h3>Why does laser-cut acrylic craze when I glue it?<\/h3>\n<p>The heat-affected zone. Cutting leaves a 0.1\u20130.3 mm layer of stressed, micro-cracked polymer along the edge, and solvent wicks into the cracks. Anneal the parts at 80 \u00b0C for about an hour per 3 mm of thickness before bonding, and cool slowly.<\/p>\n<h3>Does laser cutting weaken acrylic?<\/h3>\n<p>Locally, yes. The heat-affected zone is more brittle than the parent material and has lower resistance to impact and to solvent attack. For most display and signage work this is irrelevant; for a load-bearing or pressure part it matters, and annealing or machining the edge removes the problem.<\/p>\n<h3>Can I cut acrylic with a fibre laser?<\/h3>\n<p>No. Fibre lasers emit at about 1.06 \u00b5m, and acrylic is essentially transparent at that wavelength, so the beam passes through instead of being absorbed. Only a CO2 laser at 10.6 \u00b5m couples into PMMA.<\/p>\n<h3>Should I leave the protective film on when cutting?<\/h3>\n<p>Polyethylene film can stay on for thin sheet at reduced power, though it may melt slightly into the top edge. Paper masking should come off \u2014 it smoulders and ignites. For any cut where the edge is visible, cut bare and accept the handling risk.<\/p>\n<h3>Is laser-cut acrylic food safe?<\/h3>\n<p>The base polymer is, but the cut edge is not automatically. The heat-affected zone can retain monomer and the surface is not smooth enough to clean properly. For food-contact parts, machine and polish the edge, or use a cast sheet and anneal after cutting.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Need acrylic parts cut to a drawing?<\/p>\n<p>Send us the sheet thickness, the profile and what the edge has to look like. We will tell you whether the part belongs on a laser, a router or a saw \u2014 and what tolerance is actually achievable at that size.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ru\/acrylic-rod\/\">Talk to an acrylic fabrication engineer<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ru\/polycarbonate-vs-acrylic-tube\/\">Polycarbonate vs Acrylic Tube: Impact, Clarity and Cost<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ru\/cast-vs-extruded-acrylic-rod\/\">Cast vs Extruded Acrylic Rod: Which One to Specify<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ru\/acrylic-rod-specification-guide\/\">Acrylic Rod Sizes, Tolerances and Straightness<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ru\/storing-handling-acrylic-rod\/\">Storing and Handling Acrylic Rod Without Crazing It<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ru\/acrylic-rod-colour-consistency\/\">Acrylic Rod Colour Consistency: Batch, Light and Measurement<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>A CO2 laser is the only common process that leaves acrylic polished straight off the machine. What the beam does, why cast and extruded differ, and the design rules.<\/p>","protected":false},"author":1,"featured_media":7723,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_seopress_titles_title":"Laser Cutting Acrylic: Parameters, Edge Quality and Design R","_seopress_titles_desc":"A CO2 laser is the only common process that leaves acrylic polished straight off the machine. What the beam does, why cast and extruded differ, and the des","_seopress_robots_index":"","_seopress_robots_follow":"","_seopress_robots_imageindex":"","_seopress_robots_snippet":"","_seopress_robots_primary_cat":"38","_seopress_robots_breadcrumbs":"","_seopress_robots_freeze_modified_date":"","_seopress_robots_custom_modified_date":"","_seopress_robots_canonical":"","_seopress_social_fb_title":"","_seopress_social_fb_desc":"","_seopress_social_fb_img":"","_seopress_social_fb_img_attachment_id":0,"_seopress_social_fb_img_width":0,"_seopress_social_fb_img_height":0,"_seopress_social_twitter_title":"","_seopress_social_twitter_desc":"","_seopress_social_twitter_img":"","_seopress_social_twitter_img_attachment_id":0,"_seopress_social_twitter_img_width":0,"_seopress_social_twitter_img_height":0,"_seopress_redirections_value":"","_seopress_redirections_enabled":"","_seopress_redirections_enabled_regex":"","_seopress_redirections_logged_status":"","_seopress_redirections_param":"","_seopress_redirections_type":0,"_seopress_analysis_target_kw":"laser cutting acrylic","footnotes":""},"categories":[38],"tags":[],"class_list":["post-7731","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-acrylic-rod"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/posts\/7731","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/comments?post=7731"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/posts\/7731\/revisions"}],"predecessor-version":[{"id":7733,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/posts\/7731\/revisions\/7733"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/media\/7723"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/media?parent=7731"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/categories?post=7731"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ru\/wp-json\/wp\/v2\/tags?post=7731"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}