{"id":8276,"date":"2026-03-29T09:00:00","date_gmt":"2026-03-29T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/halogen-free-cable-compound\/"},"modified":"2026-03-29T09:00:00","modified_gmt":"2026-03-29T08:00:00","slug":"halogen-free-cable-compound","status":"publish","type":"post","link":"https:\/\/uplastech.com\/pt\/halogen-free-cable-compound\/","title":{"rendered":"Halogen-Free Cable Compounds: Filled Systems and the Extrusion They Demand"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/halogen-free-cable-compound.jpg\" alt=\"Two glass jars of pale grey cable compound pellets, one speckled with white mineral filler, a length of black cable jacket beside them on a laboratory bench\" width=\"1536\" height=\"909\"><figcaption>The same polymer with and without the filler load. Halogen-free means the second jar, and everything that follows from it.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"why\">Halogen-free is a filler story<\/h2>\n<p>A conventional PVC cable jacket gets its flame resistance from chlorine. The chlorine is part of the polymer, it is 57 percent of the weight, and it works: a PVC jacket will not sustain a flame. The problem is what it releases when it does burn, which is hydrogen chloride, and that is the reason halogen-free compounds exist.<\/p>\n<p>A halogen-free compound has no chlorine and no bromine, so it has to get its flame resistance from something else. The something is a mineral filler that decomposes endothermically: aluminium trihydroxide, which releases water at about 200 C, or magnesium dihydroxide, which does it at about 330 C. The decomposition absorbs heat and dilutes the flame with steam, and it only works if there is a lot of it.<\/p>\n<p>A lot means 55 to 65 parts per hundred of filler to 100 parts of polymer. At that loading the filler is more than a third of the compound by weight, and the compound stops behaving like a plastic and starts behaving like a filled system. That single fact explains almost everything that is difficult about running it.<\/p>\n<p>The alternative flame retardants are phosphorus-based or intumescent, and they work at 15 to 25 phr instead of 60. They are also more expensive, they are less effective in a thin wall, and they have their own smoke and toxicity profile. For a general purpose jacket the mineral route is the default.<\/p>\n<h2 id=\"strength\">What 60 phr of filler does to the properties<\/h2>\n<p>A filler is not a reinforcement at this loading. It is a diluent with a particle size of 1 to 3 micrometres, and it occupies volume that the polymer used to occupy. The polymer chains that used to be continuous are now separated by particles, and the strain at break falls because the chains have less room to extend.<\/p>\n<p>Unfilled, an EVA-based jacket compound has a tensile strength of about 16.5 MPa and an elongation at break of 420 percent. At 20 phr the strength is 13.8 and the elongation 330. At 40 phr it is 10.9 and 235. At 55 phr it is 8.6 and 160. At 65 phr it is 6.4 and 105.<\/p>\n<p>That last number is the one that matters for a cable. A jacket has to survive being bent around a drum, pulled through a duct and stripped by an electrician. An elongation of 105 percent is a jacket that will crack at a tight bend radius after a few years of thermal cycling, and it is the reason a halogen-free cable is specified with a larger bend radius than the PVC cable it replaces.<\/p>\n<p>The strength loss can be recovered partly by coupling. A silane coupling agent or a maleic anhydride grafted polymer bonds the filler to the matrix, and it buys 15 to 25 percent of the tensile strength back at the same loading. It also costs money and it makes the compound more sensitive to moisture during storage.<\/p>\n<figure>\n<img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/halogen-free-cable-compound-chart.jpg\" alt=\"Tensile strength falling from 16.5 to 6.4 MPa and elongation from 420 to 105 percent as filler loading rises from 0 to 65 phr, and head pressure rising from 95 to 340 bar over the same range\" width=\"1536\" height=\"909\"><figcaption>Left: tensile strength and elongation against filler loading, 16.5 MPa and 420 percent unfilled against 6.4 MPa and 105 percent at 65 phr. Right: head pressure over the same range, 95 bar to 340 bar, which is what the die and the screw have to handle.<\/figcaption><\/figure>\n<h2 id=\"pressure\">Head pressure is where the line feels it<\/h2>\n<p>A filled compound is far more viscous than the polymer it is based on, and viscosity shows up as pressure. At zero filler the head pressure on a typical jacket line is about 95 bar. At 20 phr it is 138, at 40 it is 196, at 55 it is 268, and at 65 it is 340.<\/p>\n<p>That is a problem for three things. The die has to be built to take it, and a die that was designed for 150 bar will deflect at 340, which shows up as an oval jacket. The screw has to be able to generate it without over-shearing the compound, and a general purpose screw on a filled compound generates heat faster than it generates pressure. The screen pack has to be changed more often, because the pressure rise across a blinded screen is larger when the baseline is already high.<\/p>\n<p>The usual answer is a barrier screw with a deeper metering section and a lower compression ratio. A 2.5:1 compression screw that works well on an unfilled polyolefin will over-compress a 60 phr compound and shear it, and a 1.8:1 screw with a longer metering zone will run it at the same output with 20 C less melt temperature rise.<\/p>\n<p>The other answer is temperature. A filled compound runs hotter because the filler conducts heat and because the viscosity dissipates more energy. A melt temperature that would be 180 C on an unfilled compound is 195 to 205 C on the filled one at the same setpoints, and the die heater bands have to be set lower to compensate.<\/p>\n<h2 id=\"die\">The die, and why it is not the same die<\/h2>\n<p>A die for a filled compound has three differences from one for an unfilled compound. The land is shorter, because a long land on a high-viscosity melt generates pressure without improving the surface. The taper is more gradual, because a filled melt is more prone to dead spots in a sharp corner, and a dead spot is a place where the filler settles out.<\/p>\n<p>The third difference is wear. Aluminium trihydroxide is abrasive, and a die running 60 phr of it at 340 bar wears at the land. A tool steel die that holds its dimensions for years on a PVC line will show 0.05 mm of land wear in a year on a filled line, and land wear changes the die swell and therefore the wall thickness.<\/p>\n<p>The die also has to be sized for a different die swell. A filled compound has less elastic recovery than an unfilled one, so it swells less at the die exit, and a die cut for the unfilled swell produces an undersized jacket. The correction is 3 to 6 percent on the die diameter, and it is measured rather than calculated.<\/p>\n<table>\n<thead>\n<tr>\n<th>Die variable<\/th>\n<th>Unfilled<\/th>\n<th>60 phr filled<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Land length<\/td>\n<td>10 to 15 x wall<\/td>\n<td>6 to 10 x wall<\/td>\n<\/tr>\n<tr>\n<td>Taper angle<\/td>\n<td>30 degrees<\/td>\n<td>15 degrees<\/td>\n<\/tr>\n<tr>\n<td>Morrer bem<\/td>\n<td>8 to 12%<\/td>\n<td>3 to 6%<\/td>\n<\/tr>\n<tr>\n<td>Land material<\/td>\n<td>Hardened steel<\/td>\n<td>Coated or carbide<\/td>\n<\/tr>\n<tr>\n<td>Head pressure<\/td>\n<td>95 to 150 bar<\/td>\n<td>270 to 340 bar<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 How the die changes for a filled compound<\/p>\n<h2 id=\"screw\">Screw, screen and the things that block<\/h2>\n<p>The screen pack on a filled line is a consumable, not a filter. A 40 mesh screen on a 60 phr compound blinds in 4 to 8 hours, and a blinded screen raises the head pressure by 40 to 60 bar before it ruptures. The rule is to change on a pressure rise of 25 bar, not on a schedule, and to log the rise so a trend is visible.<\/p>\n<p>The screw itself wears. A standard nitrided screw on a filled compound loses its flight clearance in 12 to 18 months, and a worn screw cannot build pressure, so the line runs hotter and slower to compensate. A bimetallic barrel and a hard-faced screw are not optional on a filled line; they are the difference between a screw that lasts five years and one that lasts one.<\/p>\n<p>The feed zone is the other place things block. A filled compound is more abrasive and less slippery, and it can bridge in the hopper throat. A hopper with a vibrator or a crammer feeder is standard on a filled line, and a hopper that works on pellets will starve on a 60 phr compound at high output.<\/p>\n<p>Moisture is the last one. Aluminium trihydroxide is hydrophilic, and a compound that has absorbed 0.1 percent moisture will produce voids at the die, exactly like a crosslinked polyethylene that was not dried. A dryer on the hopper is part of the line, not an accessory.<\/p>\n<table>\n<thead>\n<tr>\n<th>Symptom<\/th>\n<th>What it means<\/th>\n<th>What to change<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Head pressure climbing<\/td>\n<td>Screen blinding<\/td>\n<td>Change screen at 25 bar rise<\/td>\n<\/tr>\n<tr>\n<td>Output falling at fixed rpm<\/td>\n<td>Desgaste do parafuso<\/td>\n<td>Check flight clearance<\/td>\n<\/tr>\n<tr>\n<td>Voids in the jacket<\/td>\n<td>Moisture in the compound<\/td>\n<td>Dry the compound<\/td>\n<\/tr>\n<tr>\n<td>Oval jacket<\/td>\n<td>Die deflection<\/td>\n<td>Support the die, reduce pressure<\/td>\n<\/tr>\n<tr>\n<td>Rough surface<\/td>\n<td>Land too long, melt too cool<\/td>\n<td>Shorten the land, raise the melt<\/td>\n<\/tr>\n<tr>\n<td>Bridging in the hopper<\/td>\n<td>Poor feed<\/td>\n<td>Crammer or vibrator<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 Running a filled compound, symptom by symptom<\/p>\n<h2 id=\"choice\">When halogen-free is the wrong answer<\/h2>\n<p>A halogen-free cable is bigger, stiffer and more expensive than the PVC cable it replaces. It is bigger because the filler displaces polymer and the jacket has to be thicker to reach the same mechanical and flame performance. It is stiffer because the elongation is half. It is more expensive because the compound costs two to three times as much.<\/p>\n<p>That is a fair trade in a tunnel, a rolling stock interior, a data centre plenum or anywhere the acid gas from a PVC fire would damage equipment or people. It is a poor trade in a domestic appliance cord, where the fire load is small and the cost difference is visible on the shelf.<\/p>\n<p>The regulations that drive the choice are worth knowing. IEC 60754 covers acid gas, IEC 61034 covers smoke density, and IEC 60332-3 covers flame spread on a bundle. A compound can pass one and fail another, and a specification that says halogen-free without naming the tests is a specification that can be met by a compound that still burns.<\/p>\n<div class=\"myth\">Myth: halogen-free means flame retardant. It means no halogen. A halogen-free compound with too little filler burns cleanly and enthusiastically. The flame resistance comes from the 55 to 65 phr of mineral filler, and a compound at 30 phr is halogen-free and not flame retardant at all.<\/div>\n<div class=\"faq\">\n<h3>Why are halogen-free compounds so heavily filled?<\/h3>\n<p>Because the flame resistance comes from a mineral that decomposes endothermically, and it only works at 55 to 65 parts per hundred. Below that the compound is halogen-free but not flame retardant.<\/p>\n<h3>How much strength does the filler cost?<\/h3>\n<p>Tensile strength falls from 16.5 MPa unfilled to 6.4 MPa at 65 phr, and elongation from 420 to 105 percent. Coupling agents recover 15 to 25 percent of the strength.<\/p>\n<h3>Why does head pressure go up so much?<\/h3>\n<p>A filled melt is far more viscous. Head pressure goes from about 95 bar unfilled to 340 bar at 65 phr, which is why the die, the screw and the screen pack all have to change.<\/p>\n<h3>Can I run a filled compound on a standard screw?<\/h3>\n<p>It will run, but it will over-compress and over-shear the compound. A barrier screw with a lower compression ratio and a longer metering zone runs 20 C cooler at the same output.<\/p>\n<h3>Does a halogen-free jacket need drying?<\/h3>\n<p>Yes. Aluminium trihydroxide is hydrophilic, and 0.1 percent moisture produces voids at the die just like an undried crosslinked polyethylene.<\/p>\n<h3>Is halogen-free always the right choice?<\/h3>\n<p>No. It is bigger, stiffer and two to three times the compound cost. It is right where acid gas and smoke matter, and it is a poor trade on a domestic appliance cord.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">A halogen-free compound that will not run?<\/p>\n<p>Tell us the filler loading, the wall thickness and the output you need. We will tell you the screw, the die and the drying the compound requires.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/pt\/solucoes-de-extrusao-de-plastico\/\">Ask about cable extrusion<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/pt\/wire-insulation-extrusion\/\">Wire Insulation Extrusion: The Die, the Tip and the Wall<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pt\/cable-jacket-extrusion\/\">Cable Jacket Extrusion: Wall, Ovality and the Trough<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pt\/cable-extrusion-defects\/\">Cable Extrusion Defects: Voids, Protrusions and the Die<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pt\/cable-filler-and-shield\/\">Cable Fillers and Shields: Combining Extrusion With Taping and Braiding<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pt\/solucoes-de-extrusao-de-plastico\/\">Plastic Extrusion Solutions: Profile, Pipe and Cable<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>A halogen-free compound is 60 phr of mineral filler and 40 phr of polymer. That takes tensile strength from 16.5 to 6.4 MPa and head pressure from 95 to 340 bar, and the die has to be designed for it.<\/p>","protected":false},"author":1,"featured_media":8274,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[17],"tags":[],"class_list":["post-8276","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-plastic-extrusion-process"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/posts\/8276","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/comments?post=8276"}],"version-history":[{"count":0,"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/posts\/8276\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/media\/8274"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/media?parent=8276"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/categories?post=8276"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/pt\/wp-json\/wp\/v2\/tags?post=8276"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}