Spliced Silicone Cord That Fails at the Joint: Tensile Strength, Cure and Acceptance

Real moulded silicone seals and O-rings made by Uplastech
Real silicone rubber production context. Uplastech product photo.

The problem

Symptom. A 6 mm extruded silicone cord made into a 300 mm ring snaps at its splice during fitting, and a tensile pull returns 3.8 MPa against an 8.5 MPa parent value.

What it costs. The cord itself is in spec, yet every ring fails at one point, so a cleanroom assembly line is stopped and the splicing method is disputed.

This guide compares scarf and butt splices by tensile strength, sets a 75 % of parent limit, and gives a joint acceptance test and position clause.

Why the splice is the weak point

An extruded cord is only as strong as its splice. A 6 mm, 60 Shore A cord has a parent tensile of 8.5 MPa, yet an RTV butt splice reaches only 3.8 MPa, 45 % of parent, so the joint tears first.

Finding at the joint Most likely cause Confirming check
Clean break across the bond line Cold RTV butt splice Section the joint and tensile-test five
Tensile near 45 % of parent RTV cure, no heat Compare against the 7.2 MPa scarf value
Joint sits on the sealing land Poor joint position Measure 30 mm clearance on the drawing
Scarf holds 85 % of parent Heat-vulcanised scarf Accept against the 6.4 MPa limit

Table 1 - Reading a spliced extruded cord failure

Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.

Need a fixed price for this seal?

Send the gland drawing, temperature range, media and annual volume. We will recommend a compound with test data and return samples with a written production quotation.

Get a silicone seal quotationEmail [email protected]WhatsApp

Test splice tensile against the parent cord

Pull five splices and five parent samples per lot to ISO 37 at 100 mm/min, and log the joint position. The chart below plots splice tensile against cure time at 180 C for scarf and butt joints, against a 6.4 MPa limit.

A five-step diagnostic sequence

  1. Locate and mark the joint.
    Record its clock position and distance to the sealing land on the rejected ring.
  2. Tensile-test five splices and five parent samples.
    Pull to ISO 37 at 100 mm/min and 23 C; express the splice as a percentage of parent.
  3. Section one failed joint.
    A smooth bond line indicates an RTV butt splice; a continuous phase indicates a heat-vulcanised scarf.
  4. Run a 180-degree bend on a 25 mm mandrel.
    Any crack at the scarf fails the joint regardless of the tensile figure.
  5. Agree the acceptance clause.
    Specify 6.4 MPa minimum, 75 % of parent, 20 mm scarf and a 30 mm land clearance.

The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

Spliced Silicone Cord That Fails at the Joint: Tensile Strength, Cure and Acceptance: calculated response trend and an illustrative root-cause split
Figure 1 — Calculated response trend and an illustrative root-cause split. Values are engineering guidance for diagnosis, not a measured survey; confirm them on your own line before changing a drawing or a specification.

Specify the scarf joint and its cure

Specify a 20 mm scarf joint heat-vulcanised with uncured tape at 180 C for 10 min under 2 bar, reaching 7.2 MPa, 85 % of parent. Locate it in a straight run at least 30 mm from any sealing land.

Parâmetro Typical target What goes wrong outside it
Splice type 20 mm scarf, heat-vulcanised An RTV butt joint reaches only 45 % of parent
Cure condition 180 C, 10 min, 2 bar A cold cure leaves 3.8 MPa tensile
Splice tensile strength Above 6.4 MPa (75 % of parent) Below 6.4 MPa the joint tears first
Joint position 30 mm from any sealing land A joint on the land leaks in service

Table 2 - Splice and acceptance parameters to put on the order

Set a joint acceptance test

Write a joint acceptance test into the order: minimum 75 % of parent tensile, or 6.4 MPa, plus a 180-degree bend round a 25 mm mandrel with no crack at the scarf. Require five splices and five parent samples tested per lot at 23 C.

Option When it fits Trade-off
Re-splice with a 180 C scarf joint Cold RTV splice found Rework labour and a heated press
Move the joint to a straight run Joint on a sealing land Ring orientation must be controlled
Raise cure to 10 min at 2 bar Under-cured heat splice Longer cycle per joint
Write a 75 % tensile clause Future orders Narrower splice options

Table 3 - Corrective paths for a failed cord splice

Myth: "A process adjustment will fix it." Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.

Read the failed joint under section

Confirm the fix by sectioning one rejected ring: an RTV butt splice shows a smooth bond line, a heat-vulcanised scarf a continuous rubber phase. A joint that cracks on the 25 mm mandrel also sits below 3.8 MPa in tension.

Want a compound check before you re-order?

Send us the gland drawing and the service conditions. We will compare the compound data against your temperature range and return a recommendation with sample parts.

What to send us

  • Gland dimensions and cross-section
  • Temperature range and media
  • A failed seal if available
  • Annual volume

Send the gland drawing

Close the claim with a lot tensile record

Recover the held batch by re-splicing twenty rings with the 180 C scarf and re-testing five splices per lot. If tensile stays below 6.4 MPa, quarantine the lot; never accept a cold RTV splice.

Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.

Before you release this silicone seal

  • A 20 mm scarf joint cured at 180 C for 10 min under 2 bar is specified
  • Splice tensile above 6.4 MPa, or 75 % of parent, is in the purchase order
  • The joint is located at least 30 mm from any sealing land or corner
  • Five splices and five parent samples are tensile-tested per lot at 23 C
  • A 180-degree bend round a 25 mm mandrel is part of the acceptance test

Most cold or heat failures are specification gaps, not bad batches. Fix the specification before changing suppliers.

Why does the cord always break at the splice?

The joint is the weakest section. A 6 mm, 60 Shore A cord has 8.5 MPa parent tensile, but an RTV butt splice reaches only 3.8 MPa, 45 % of parent.

Which splice method should we specify?

A 20 mm scarf joint heat-vulcanised with uncured tape at 180 C for 10 min under 2 bar. It reaches 7.2 MPa, 85 % of parent tensile.

What tensile limit is realistic?

Above 6.4 MPa, or 75 % of parent. Test five splices and five parent samples per lot to ISO 37 at 100 mm/min.

Does joint position matter?

Yes. Keep the splice in a straight run at least 30 mm from any sealing land or corner, so assembly stretch and pressure never load it directly.

How do we tell an RTV splice from a heat splice?

Section the joint. An RTV butt splice shows a smooth bond line; a heat-vulcanised scarf shows a continuous rubber phase with no interface.

Can a cold splice be accepted?

No. A joint that cracks on the 25 mm mandrel also sits below 3.8 MPa in tension. Re-splice with the 180 C scarf and re-test per lot.

Get a seal specified for the real service conditions

Send us the gland drawing and the service conditions. We will recommend a compound with documented test data, review the squeeze, and supply samples with a production quotation.

To get an accurate quote, send:

  • Gland drawing or seal cross-section
  • Temperature range and media
  • Pressure and movement
  • Annual volume and target unit price

Request samples and a quotation

Prefer to talk it through first?

Correio eletrónico [email protected] or message us on WhatsApp +86 177 1752 9949. Send a drawing, a sample or a specification and an engineer will reply.

Why buyers work with Uplastech

ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
pt_PTPT

Pedir um orçamento rápido

Enviar desenhos e requisitos pormenorizados através de

Emial: [email protected]

Ou preencha o formulário de contacto abaixo: