
The problem
Symptom. After a cold start the open gate drools a 12 mm string of ABS from a tip zone held at 255 C against a 240 C manifold, and the first 10 parts carry the witness mark.
What it costs. Stringing marks the A-surface of the first parts after every start, so start-up scrap repeats after each break and the moulder and buyer argue over who owns the purge shots and the quarantined parts.
This guide ties stringing to tip temperature offset and decompression, then gives the setpoints, purge shot count and first-parts quarantine to write into the start-up procedure.
What tip stringing looks like at start-up
Stringing is the opposite of a cold slug. A tip zone held at 255 C against a 240 C manifold keeps the gate molten and drools a 12 mm ABS string, while a 230 C tip with 5 mm decompression leaves under 2 mm.
| Observed symptom | Most likely cause | First check on the line |
|---|---|---|
| 12 mm string from an open gate | Tip 15 C above the manifold | Read the tip and manifold thermocouples |
| String shrinks over the first 8 shots | Tip cooling from 255 to 230 C | Log drool length by shot number |
| String returns after every idle | Stand-by tip held too hot | Check the stand-by setpoint against running |
| Dark blemish on shot 1 instead | Cold slug, not drool | Check soak time and a cold-slug well |
Table 1 - Reading start-up stringing before changing the heater
Need a fixed price for this moulded part?
Send the 2D drawing, resin grade and annual volume. Our engineers return a DFM review, a material recommendation and a written quotation you can compare line by line.
Separate an overheated tip from a cold slug
Read every tip thermocouple and log drool length over 8 start-up shots. Strings that shrink as the tip cools from 255 to 230 C are heat; a blocked gate or dark blemish on shot 1 is a cold slug.
A five-step diagnostic sequence
- Read every tip and manifold thermocouple.
Confirm the tip is 230 C against a 240 C manifold; a 255 C tip explains the 12 mm string. - Log drool length over 8 start-up shots.
A string that shrinks as the tip cools to 230 C is heat, not a cold slug. - Check decompression and stand-by settings.
A 2 mm stroke leaves melt at the orifice; set 5 mm and keep stand-by within 30 C of running. - Purge 8 shots after a 20 min soak.
Collect no part until the gate string reads under 3 mm at the setpoint. - Quarantine the first 10 parts and release.
Hold them after every cold start or colour change, then re-check the gate string.
The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.

Tip and decompression setpoints for the sheet
Put the balance on the process sheet: manifold 240 C, tip 230 C, so 10 C below, stand-by no more than 30 C below running, 5 mm decompression and 8 purge shots before any part is collected.
| Parâmetro | Typical target | What goes wrong outside it |
|---|---|---|
| Tip temperature for ABS | 230 C, 10 C below a 240 C manifold | At 255 C the gate drools a 12 mm string |
| Decompression (suck-back) stroke | 5 mm | At 2 mm melt stays at the orifice |
| Start-up purge shots | 8 at setpoint | Too few leave strings on the first parts |
| Stand-by idle setpoint | Within 30 C below running | Holding the tip 15 C hot grows drool |
Table 2 - Hot-runner parameters for the process sheet
Temperature balance and purge that clear drool
A 2 mm decompression stroke leaves melt at the orifice and strings 12 mm; 5 mm pulls it back. Holding the tip 15 C above the manifold during idle also grows a drool that no purge volume can fully remove.
| Controlo | Effect on the string | Trade-off |
|---|---|---|
| Set tip 230 C, 10 C below manifold | Drool falls from 12 to under 2 mm | Tip must be re-balanced per grade |
| Raise decompression 2 to 5 mm | Pulls melt back from the orifice | Too much can draw air into the gate |
| Purge 8 shots before collecting | Clears degraded melt | 8 shots of start-up scrap per start |
| Quarantine the first 10 parts | Keeps string-marked parts out | 10 parts held after every cold start |
Table 3 - Controls that remove start-up drool
Write a purge and quarantine rule into the order
Agree start-up acceptance before first article: drool string of at most 3 mm at the gate, 8 purge shots at setpoint, a 20 min soak and the first 10 parts quarantined after every cold start or colour change.
Not sure whether the fault is in the tool or the process?
Send us the drawing, the process window and a few sample parts. We will tell you which change fixes the fault before you commit to a tool modification.
What to send us
- Part drawing with the affected dimension
- Current process settings
- Sample parts from a good and a bad batch
- Annual volume
Recovery actions ranked by start-up disruption
On a running line, lower the tip to 230 C, set 5 mm decompression and purge 8 shots before sampling. Quarantine the first 10 parts, then release only when the gate string reads under 3 mm.
Before you release this injection moulding job
- Manifold at 240 C and tip at 230 C are named in the process sheet, 10 C apart
- Decompression stroke of 5 mm and a stand-by within 30 C of running are specified
- A 20 min soak and 8 purge shots at setpoint are written into the start-up procedure
- A maximum gate string of 3 mm is agreed before first article
- The first 10 parts are quarantined after every cold start and colour change
Attach this list to the RFQ. Most moulding faults are decided at the drawing stage.
Is stringing the same as a cold slug?
No. A cold slug is a solid plug from a tip at 200 C; stringing is molten drool from a tip at 255 C against a 240 C manifold, leaving a 12 mm string.
Why does the tip run cooler than the manifold?
A tip about 10 C below the 240 C manifold lets the gate skin freeze between shots. At 255 C it stays molten and drools.
How much decompression is enough?
A 5 mm suck-back stroke pulls melt off the orifice; a 2 mm stroke leaves 12 mm of string. Too much can draw air, so stay near 5 mm.
How many purge shots do we need?
Eight shots at setpoint after a 20 min soak clears the degraded melt. Write the 8 shots and the first 10 quarantined parts into the order.
Why does drool return after a colour change?
During idle the stand-by tip is held too hot. Keep stand-by within 30 C of running, re-balance to 230 C and purge 8 shots before sampling.
Who owns the start-up scrap?
Agree it up front. Name the soak, the 8 purge shots, the 3 mm string limit and the first 10 quarantined parts so each start is judged by one rule.
Get a mouldable part and a fixed quotation
Send us the part file and the failure history. Our engineers will return a DFM review, a material recommendation and a fixed quotation with a defined first-article acceptance test.
To get an accurate quote, send:
- 3D file or 2D part drawing
- Resin grade and any regrind limit
- Annual volume and target unit price
- The failed sample or defect photos
Request a DFM review and quote
Prefer to talk it through first?
Correio eletrónico [email protected] or message us on WhatsApp +86 177 1752 9949. Send a drawing, a sample or a specification and an engineer will reply.
Why buyers work with Uplastech
ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.