{"id":10311,"date":"2026-11-20T01:00:00","date_gmt":"2026-11-20T01:00:00","guid":{"rendered":"https:\/\/uplastech.com\/?p=10311"},"modified":"2026-11-17T12:51:31","modified_gmt":"2026-11-17T12:51:31","slug":"injection-household-kitchenware-rib-sink-marks","status":"publish","type":"post","link":"https:\/\/uplastech.com\/pl\/injection-household-kitchenware-rib-sink-marks\/","title":{"rendered":"Sink Marks Over Ribs on Kitchenware Lids After the Gloss Coat"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n\/* ==UPL-CONVERSION-MODULES-START== 2024 problem-solving \/ lead-gen blocks *\/\n.upl-blog .mod-h{font-size:12.5px;letter-spacing:.12em;text-transform:uppercase;font-weight:700;color:#0d5563;margin:0 0 12px}\n.upl-blog .problem{background:#fff8f3;border:1px solid #f3ddc9;border-left:4px solid #e07a1f;border-radius:10px;padding:22px 26px;margin:0 0 32px;font-size:16px}\n.upl-blog .problem p{margin:0 0 10px}\n.upl-blog .problem p:last-child{margin-bottom:0}\n.upl-blog .problem .mod-h{color:#a85c10}\n.upl-blog .problem .problem-promise{font-weight:700;color:#0b2b33}\n.upl-blog .steps{background:#f7fafb;border:1px solid #e1ebee;border-radius:10px;padding:22px 26px;margin:0 0 28px}\n.upl-blog .steps ol{list-style:none;counter-reset:uplst;margin:0;padding:0}\n.upl-blog .steps li{counter-increment:uplst;position:relative;padding:0 0 16px 42px;margin:0;font-size:15.5px}\n.upl-blog .steps li:last-child{padding-bottom:0}\n.upl-blog .steps li::before{content:counter(uplst);position:absolute;left:0;top:2px;width:26px;height:26px;border-radius:50%;background:#0d5563;color:#fff;font-size:13px;font-weight:700;line-height:26px;text-align:center}\n.upl-blog table.spec th{background:#14707f}\n.upl-blog .conv{background:#eef6f7;border:1px solid #cfe4e8;border-radius:10px;padding:24px 26px;margin:32px 0}\n.upl-blog .conv p{margin:0 0 12px;font-size:15.5px}\n.upl-blog .conv .conv-lbl{font-weight:700;color:#0b2b33;margin:16px 0 8px}\n.upl-blog ul.conv-need{list-style:none;padding:0;margin:0 0 20px;display:grid;grid-template-columns:1fr 1fr;gap:6px 18px}\n.upl-blog ul.conv-need li{position:relative;padding-left:20px;margin:0;font-size:14.5px}\n.upl-blog ul.conv-need li::before{content:\"\";position:absolute;left:0;top:9px;width:9px;height:9px;border:2px solid #14707f;border-radius:2px}\n.upl-blog .conv-btn{display:inline-block;background:#0d5563;color:#fff;text-decoration:none;font-weight:700;padding:11px 22px;border-radius:7px;font-size:15px}\n.upl-blog .checklist{background:#fbfcfd;border:1px solid #e3e9ec;border-radius:10px;padding:24px 26px;margin:36px 0}\n.upl-blog .checklist ul{list-style:none;padding:0;margin:0 0 12px}\n.upl-blog .checklist li{position:relative;padding-left:28px;margin:0 0 10px;font-size:15.5px}\n.upl-blog .checklist li::before{content:\"\";position:absolute;left:0;top:7px;width:14px;height:14px;border:2px solid #0d5563;border-radius:3px}\n.upl-blog .cl-note{font-size:13.5px;color:#6b7280;margin:0}\n.upl-blog .cta .cta-lbl{color:#c9dee3;font-weight:700;margin:0 0 8px;font-size:14.5px}\n.upl-blog ul.cta-need{list-style:none;padding:0;margin:0 0 22px;display:grid;grid-template-columns:1fr 1fr;gap:4px 18px}\n.upl-blog ul.cta-need li{color:#e4f0f2;font-size:14.5px;padding-left:18px;position:relative;margin:0}\n.upl-blog ul.cta-need li::before{content:\"\\2713\";position:absolute;left:0;color:#e07a1f;font-weight:700}\n\/* ==UPL-CONVERSION-MODULES-END== *\/\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}.upl-blog ul.conv-need,.upl-blog ul.cta-need{grid-template-columns:1fr}.upl-blog .problem,.upl-blog .steps,.upl-blog .conv,.upl-blog .checklist{padding:18px}}\n\/* Single-post: hide the greeting card, keep the round WhatsApp bubble.\n   The Click to Chat logic refuses to open a chat while the greeting node exists,\n   so Code Snippets #9 removes that node from the DOM. This rule is only the visual fallback.\n   Delete #9 before removing this rule. *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure><img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/2024-resin-grade-last-time-buy-notice-moulding-hero-scaled.jpg\" alt=\"Sink Marks Over Ribs on Kitchenware Lids After the Gloss Coat\" \/><figcaption>Injection moulding: a production part is the only useful reference for a discussion about process drift.<\/figcaption><\/figure>\n<p class=\"lead\">A shallow depression shows over each reinforcing rib once a kitchenware lid is painted, even though the bare moulding looked flat.<\/p>\n<div class=\"toc\"><\/div>\n<h2 id=\"what\">What the failure looks like on the line<\/h2>\n<p>High-volume household parts are audited on cosmetics and fit across long runs, so a slow process drift is more expensive than a single bad shot.<\/p>\n<p>Faint depressions appear on the visible face directly above internal ribs, and a subsequent high-gloss finish makes them obvious. The wall thickness elsewhere is unchanged.<\/p>\n<p>A rib thicker than the nominal wall cools more slowly and shrinks more, pulling the skin inward to leave a sink mark on the opposite face. Low holding pressure or an early gate freeze stops compensation of that local shrinkage. A glossy coating amplifies the shallow depression by specular reflection, a behaviour often called rib telegraphing after paint.<\/p>\n<p>Most of these complaints arrive after the parts have been accepted, which is a sign that the acceptance test measured the wrong thing. On a buyer's specification this distinction matters: a part can measure inside tolerance and still fail in use, because the drawing records geometry while the complaint records behaviour. Rib-to-wall thickness ratio is usually the first value both sides compare, and it is also the one most often quoted without the conditions attached to it.<\/p>\n<h2 id=\"window\">The process window that decides it<\/h2>\n<p>Four variables move this result more than the rest. The ranges below are illustrative engineering guidance for a first discussion; confirm them on your own tool, material grade and part geometry before they become contract terms.<\/p>\n<table>\n<thead>\n<tr>\n<th>Zmienna<\/th>\n<th>Typical window<\/th>\n<th>What fails outside it<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Rib-to-wall thickness ratio<\/td>\n<td>0.5-0.7<\/td>\n<td>Above the window the rib sinks the face opposite<\/td>\n<\/tr>\n<tr>\n<td>Holding pressure<\/td>\n<td>60-90 MPa<\/td>\n<td>Low holding cannot compensate local rib shrinkage<\/td>\n<\/tr>\n<tr>\n<td>Holding time<\/td>\n<td>5-12 s<\/td>\n<td>Too short lets the gate freeze before the rib is packed<\/td>\n<\/tr>\n<tr>\n<td>Mould temperature<\/td>\n<td>40-70 C<\/td>\n<td>Uneven tool temperature changes the sink depth across the lid<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1. Starting window for a joint process trial. Values are engineering guidance, not a measured survey.<\/p>\n<p><b>Rib-to-wall thickness ratio<\/b> is typically held at 0.5-0.7. Above the window the rib sinks the face opposite Record it together with the measurement point and the moment in the cycle; a single number without a location is not a process setting.<\/p>\n<p><b>Holding pressure<\/b> is typically held at 60-90 MPa. Low holding cannot compensate local rib shrinkage When this drifts, the symptom usually appears at one cavity, one sheet position or one lane before it appears across the whole batch.<\/p>\n<p><b>Holding time<\/b> is typically held at 5-12 s. Too short lets the gate freeze before the rib is packed A change here is cheap during a trial and expensive after tooling release, so treat it as a controlled variable with a documented re-approval.<\/p>\n<p><b>Mould temperature<\/b> is typically held at 40-70 C. Uneven tool temperature changes the sink depth across the lid Put it on the change-control list, otherwise an unannounced material or setting substitution will be mistaken for ordinary process noise.<\/p>\n<h2 id=\"response\">Reading the response curve<\/h2>\n<figure><img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/injection-household-kitchenware-rib-sink-marks-chart.jpg\" alt=\"Sink Marks Over Ribs on Kitchenware Lids After the Gloss Coat: Sink depth (relative index) against Holding time (s)\" \/><figcaption>Figure 1. Left: Sink depth (relative index) against Holding time (s). Right: how audited failures of this type typically split by cause. All plotted values are illustrative engineering guidance, not a measured survey.<\/figcaption><\/figure>\n<p>The left panel shows sink depth (relative index) as holding time (s) increases: the response falls from 90 to 14 on the illustrative 0&ndash;100 scale. The dashed line at 60 marks a proposed acceptance limit, not a universal standard. Move that line only after the test method and the sample plan have been agreed, otherwise two suppliers can both be compliant and still deliver different parts.<\/p>\n<p>Read the shape rather than a single point. A curve that changes quickly near the limit is more sensitive to ordinary process noise than one that approaches it gradually, and that difference should be reflected in how tightly the setting is controlled and how often it is checked.<\/p>\n<h2 id=\"causes\">Where the causes actually sit<\/h2>\n<p>The right panel of Figure 1 splits audited failures of this type into five groups. The percentages are illustrative engineering guidance for prioritising an investigation, not a measured survey and not a prediction for your line.<\/p>\n<table>\n<thead>\n<tr>\n<th>Przyczyna<\/th>\n<th>Illustrative share<\/th>\n<th>First check<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Rib thicker than the wall<\/td>\n<td>34%<\/td>\n<td>Measure the rib thickness against the nominal wall at several sections.<\/td>\n<\/tr>\n<tr>\n<td>Low holding pressure<\/td>\n<td>24%<\/td>\n<td>Compare sink depth before and after the gloss finish.<\/td>\n<\/tr>\n<tr>\n<td>Early gate freeze<\/td>\n<td>18%<\/td>\n<td>Extend holding time in small steps and re-grade the visible face.<\/td>\n<\/tr>\n<tr>\n<td>Uneven mould temperature<\/td>\n<td>14%<\/td>\n<td>Check gate freeze by weighing parts across a holding-time sweep.<\/td>\n<\/tr>\n<tr>\n<td>Gloss finish amplifying the sink<\/td>\n<td>10%<\/td>\n<td>Grade the face under the same raking light as the agreed limit sample.<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2. Cause split and the corresponding first check. Shares are indicative and sum to 100.<\/p>\n<p><b>Rib thicker than the wall<\/b> accounts for roughly 34% of the illustrative split. Measure the rib thickness against the nominal wall at several sections. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.<\/p>\n<p><b>Low holding pressure<\/b> accounts for roughly 24% of the illustrative split. Compare sink depth before and after the gloss finish. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.<\/p>\n<p><b>Early gate freeze<\/b> accounts for roughly 18% of the illustrative split. Extend holding time in small steps and re-grade the visible face. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.<\/p>\n<h2 id=\"checks\">Checks before sign-off<\/h2>\n<p>The order matters because each step removes a class of explanation before the next one is opened.<\/p>\n<ol>\n<li>Measure the rib thickness against the nominal wall at several sections.<\/li>\n<li>Compare sink depth before and after the gloss finish.<\/li>\n<li>Extend holding time in small steps and re-grade the visible face.<\/li>\n<li>Check gate freeze by weighing parts across a holding-time sweep.<\/li>\n<li>Grade the face under the same raking light as the agreed limit sample.<\/li>\n<\/ol>\n<p>Keep a retained reference sample beside every result. When a batch is disputed, the comparison that settles it is almost always between the retained part and the current one under the same method, not between either part and a number on a drawing. Record the instrument, the operator, the conditioning time and the position on the part or sheet for each reading.<\/p>\n<h2 id=\"specification\">Writing it into the specification and the evidence pack<\/h2>\n<p>The visible face shall be graded for sink depth against a signed limit sample under defined raking light after finishing; a depression beyond the sample is rejectable, and the rib-to-wall ratio shall be verified on a sectioned first-off part.<\/p>\n<p>Write the requirement as a behaviour at a stated condition, not as a brand of material or a machine setting. State the test method, the conditioning, the sample plan and the rule for deciding a pass. Where a document is needed, ask the supplier for documentation that covers the actual construction and check its scope against your own market before approval; a document for the base material alone does not describe the finished part you are buying.<\/p>\n<p>At first-article approval, freeze the drawing revision, the material and colour identification, the process window, the tool and cavity identification, and the inspection method. Any later change to grade, site, tool, or window should trigger a new first article rather than a paper waiver. Keep retained samples from the approved lot and from each production lot so that a future comparison is possible.<\/p>\n<table>\n<thead>\n<tr>\n<th>Evidence item<\/th>\n<th>What it must show<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Approved drawing and revision<\/td>\n<td>The exact geometry and tolerances the decision applies to<\/td>\n<\/tr>\n<tr>\n<td>Material and colour identification<\/td>\n<td>Grade, supplier, colour reference and any declared recycled content<\/td>\n<\/tr>\n<tr>\n<td>Process window and change log<\/td>\n<td>The agreed settings and any deviation since approval<\/td>\n<\/tr>\n<tr>\n<td>Inspection record and retained samples<\/td>\n<td>Method, conditions, results and a physical reference from the same lot<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3. Minimum evidence pack for a first-article decision and a later batch dispute.<\/p>\n<p>The values quoted here are illustrative engineering guidance, not a measured survey. Agree the test method, the sample size and the acceptance rule before comparing numbers across suppliers.<\/p>\n<div class=\"faq\">\n<h2 id=\"questions\">Questions buyers ask<\/h2>\n<h3>Is this a material problem or a process problem?<\/h3>\n<p>A rib thicker than the nominal wall cools more slowly and shrinks more, pulling the skin inward to leave a sink mark on the opposite face. Low holding pressure or an early gate freeze stops compensation of that local shrinkage. A glossy coating amplifies the shallow depression by specular reflection, a behaviour often called rib telegraphing after paint. It is worth separating the two before a supplier changes a grade: hold the material constant for one controlled run, then move one setting at a time. If the symptom follows the setting, the material was never the cause.<\/p>\n<h3>Can rib-to-wall thickness ratio be traded against cycle time?<\/h3>\n<p>Only within the window stated in Table 1, and only with a recorded trial. Above the window the rib sinks the face opposite A faster cycle that sits outside the window usually moves the failure downstream, where it costs more to find.<\/p>\n<h3>What should be recorded at incoming inspection?<\/h3>\n<p>Keep the measurement, the method, the sample identity and the conditions together. Measure the rib thickness against the nominal wall at several sections. A result without its conditions cannot be compared with a later batch.<\/p>\n<h3>Does a change of household require re-approval?<\/h3>\n<p>Treat any change to material grade, tool, site or process window as a change that needs a new first-article decision. For injection moulding work the drawing alone is not enough; the process route is part of what was approved.<\/p>\n<h3>How many samples are enough for a first-article decision?<\/h3>\n<p>There is no universal number. Sample across cavities, lanes, sheet positions or reel lengths so that the spread is visible, not just the average. Agree the sample plan and the acceptance rule with the supplier before the trial starts.<\/p>\n<h3>What belongs in the evidence pack?<\/h3>\n<p>The approved drawing and revision, the material and colour identification, the process window, the inspection method and results, the retained reference samples, and documentation covering the actual construction. Ask the supplier to state the scope of each document and check it against your own market.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Seeing this on a current injection moulding job?<\/p>\n<p>Send the drawing, the material and grade, the process window you are running, and the point in the cycle or the shelf life where the fault appears. We will help you separate a material question from a process question and a specification question before anyone changes a tool.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/pl\/kontakt\/\">Talk to our injection moulding team<\/a><\/p>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/pl\/sink-marks-injection-molding\/\">Sink Marks in Injection Molding: Ribs, Bosses and the Packing That Cannot Reach<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pl\/rib-design-injection-molding\/\">Rib Design: Stiffness Without Sink, Warp or a Stuck Part<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pl\/rib-sink-telegraphing-after-paint\/\">Rib Sink Telegraphing Through Paint: Why a Flat Panel Shows Its Bones<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pl\/injection-packing-pressure-profile\/\">Packing Pressure Profile: The Setting That Decides Weight and Sink<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pl\/packing-pressure-hold-time\/\">Packing Pressure and Hold Time: How to Set Them From the Part<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>A shallow depression shows over each reinforcing rib once a kitchenware lid is painted, even though the bare moulding looked flat.<\/p>","protected":false},"author":1,"featured_media":9638,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[35],"tags":[],"class_list":["post-10311","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-injection-molding"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/posts\/10311","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/comments?post=10311"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/posts\/10311\/revisions"}],"predecessor-version":[{"id":12011,"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/posts\/10311\/revisions\/12011"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/media\/9638"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/media?parent=10311"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/categories?post=10311"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/pl\/wp-json\/wp\/v2\/tags?post=10311"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}