{"id":8047,"date":"2026-01-20T09:00:00","date_gmt":"2026-01-20T09:00:00","guid":{"rendered":"https:\/\/uplastech.com\/pc-sheet-extrusion\/"},"modified":"2026-11-01T15:26:39","modified_gmt":"2026-11-01T15:26:39","slug":"pc-sheet-extrusion","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ko\/pc-sheet-extrusion\/","title":{"rendered":"Polycarbonate Sheet: It Punishes Heat Twice"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/pc-sheet-extrusion.jpg\" alt=\"Stack of thick clear polycarbonate sheets on a steel rack, cut edges glowing amber, protective film partly peeled\" width=\"1536\" height=\"909\"><figcaption>Clear polycarbonate with its characteristic amber cut edge. The colour is not a coating, it is the material telling you how much heat it has seen.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"twice\">Heat attacks polycarbonate from two directions<\/h2>\n<p>Polycarbonate is a condensation polymer, like PET, and it hydrolyses. Water at melt temperature breaks the carbonate linkages, the molecular weight falls, and the sheet loses impact strength in a way that is not visible until something hits it. That is the first punishment, and it comes from moisture.<\/p>\n<p>The second punishment is oxidation. Polycarbonate at 320 C and above reacts with oxygen, and the reaction produces coloured species that show up as yellow. The yellowness is cumulative with time and temperature, so a resin that passes at 300 C for two minutes will fail at 340 C for two minutes, and the same resin will fail at 300 C if the residence time is long enough.<\/p>\n<p>Both failures are permanent and both are invisible in the finished sheet until the customer looks at it in daylight or drops it. That combination is what makes polycarbonate a material that rewards discipline and punishes shortcuts more than most.<\/p>\n<h2 id=\"yellow\">Twenty degrees roughly doubles the yellow<\/h2>\n<p>Yellowness index against melt temperature: 1.2 at 280 C, 2.0 at 300, 3.8 at 320, 7.5 at 340 and 14.0 at 360. A yellowness index of about 3 is where a clear sheet starts to read as slightly warm rather than clear, so the practical ceiling is around 310 C.<\/p>\n<p>The rise is faster than linear and it is roughly a doubling per twenty degrees, which is the same Arrhenius behaviour that governs the hydrolysis. The two mechanisms are not independent: wet resin hydrolyses faster at higher temperature, and the same heat that drives hydrolysis also drives oxidation.<\/p>\n<p>The trap is residence time. A barrel set at 320 C with a short residence time can produce less yellow than a barrel at 300 C with a long one, because the reaction integrates over time. That is why a small machine running a large shot, or a line stopped with the barrel full, produces yellow sheet that nobody can explain from the temperature setting alone.<\/p>\n<figure>\n<img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/pc-sheet-extrusion-chart.jpg\" alt=\"Yellowness index against melt temperature, and drying time against drying temperature\" width=\"1536\" height=\"909\"><figcaption>Yellowness runs from 1.2 at 280 C to 14 at 360 C, while drying to 200 ppm takes eight hours at 100 C and two at 130 C.<\/figcaption><\/figure>\n<h2 id=\"drying\">Drying is a time-temperature trade with a ceiling<\/h2>\n<p>Time to reach 200 ppm against drying temperature: 8 hours at 100 C, 5 at 110, 3 at 120 and 2 at 130. The trade looks free until you notice that polycarbonate softens and sticks at around 140 C, and that a hopper drier running at 130 C is close enough to that ceiling to be a risk on a hot day.<\/p>\n<p>The usual compromise is 120 C for 3 to 4 hours, which reaches the moisture target with margin and stays clear of the sticking range. Below 100 C the drying takes most of a shift and the resin may never reach 200 ppm, because the diffusion rate through a pellet falls faster than the temperature does.<\/p>\n<table>\n<thead>\n<tr>\n<th>Drying temperature<\/th>\n<th>Time to 200 ppm<\/th>\n<th>\uc704\ud5d8<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>100 C<\/td>\n<td>8 hours<\/td>\n<td>Slow, and the hopper holds a shift of resin<\/td>\n<\/tr>\n<tr>\n<td>110 C<\/td>\n<td>5 hours<\/td>\n<td>Workable on a three-shift pattern<\/td>\n<\/tr>\n<tr>\n<td>120 C<\/td>\n<td>3 hours<\/td>\n<td>The usual choice<\/td>\n<\/tr>\n<tr>\n<td>130 C<\/td>\n<td>2 hours<\/td>\n<td>Close to the sticking range<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 Drying polycarbonate: time against temperature, and the risk at each level<\/p>\n<h2 id=\"edge\">The amber edge is a measurement, not a defect<\/h2>\n<p>A cut edge of polycarbonate looks amber even when the face is clear, and the effect is stronger on a thick sheet. It is not contamination. It is the light path: looking at the edge, you are looking through 3 or 4 mm of material rather than 0.5 mm, so the intrinsic absorption of the polymer is multiplied by the distance.<\/p>\n<p>That makes the edge a free thickness gauge and a free quality indicator. Two sheets of the same nominal thickness with visibly different edge colour have seen different heat histories, and the darker one is the one that has lost more molecular weight. It is a crude measurement and it is available to anyone on the shop floor.<\/p>\n<p>The same effect explains why a formed part looks different at a corner than on a flat face. The corner is thicker after forming, so it reads darker. A customer who compares a corner to a face and reports a colour mismatch is describing geometry, not a batch problem.<\/p>\n<h2 id=\"window\">The window between too wet and too hot<\/h2>\n<p>Polycarbonate's process window is narrower than its data sheet suggests. Too wet and the chain breaks; too hot and it yellows; too long at temperature and it does both. The window that works is roughly 280 to 310 C melt, 200 ppm moisture or below, and a residence time under five minutes.<\/p>\n<table>\n<thead>\n<tr>\n<th>Symptom<\/th>\n<th>\uc6d0\uc778<\/th>\n<th>Fix<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Yellow sheet<\/td>\n<td>Melt temperature or residence time<\/td>\n<td>Lower the profile, check the shot size against the barrel<\/td>\n<\/tr>\n<tr>\n<td>Hazy sheet<\/td>\n<td>Moisture above 200 ppm<\/td>\n<td>Check dew point, drying time and hopper seals<\/td>\n<\/tr>\n<tr>\n<td>Brittle sheet, no visible defect<\/td>\n<td>Hydrolysis, molecular weight lost<\/td>\n<td>Dry harder, lower the melt temperature<\/td>\n<\/tr>\n<tr>\n<td>Silver streaks on the surface<\/td>\n<td>Moisture flashing at the die<\/td>\n<td>Dry the resin, check for a cold hopper<\/td>\n<\/tr>\n<tr>\n<td>Gels and black specks<\/td>\n<td>Degraded material held in the barrel<\/td>\n<td>Purge, check for dead spots in the flow path<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 PC sheet defects and the setting behind each<\/p>\n<p>The most common mistake is fixing a yellow sheet by lowering the temperature without checking the residence time. If the barrel is oversized for the shot, the material is sitting in it for eight minutes and no temperature will save it. The fix is a smaller barrel or a larger shot, not a colder one.<\/p>\n<h2 id=\"specify\">What to specify<\/h2>\n<p>A polycarbonate sheet specification has to carry the numbers that predict the two failures.<\/p>\n<ul>\n<li>Yellowness index, with a maximum, measured on the sheet rather than on the resin.<\/li>\n<li>Moisture at the hopper, in ppm, with the drying schedule that achieves it.<\/li>\n<li>Melt temperature and residence time, as a pair, because neither is meaningful alone.<\/li>\n<li>Impact strength after forming, since hydrolysis shows up there before it shows anywhere else.<\/li>\n<li>Which face carries the protective film, and whether the film survives the forming temperature.<\/li>\n<\/ul>\n<p>The impact test is the one that catches the invisible failure. A sheet that has lost 30 percent of its molecular weight still looks clear, still measures the right thickness, and fails on the first impact in service.<\/p>\n<div class=\"myth\">Myth: if the sheet is clear, it is good. Clarity is a measure of haze, not of molecular weight. A hydrolysed polycarbonate sheet is perfectly clear and has lost the impact strength the customer is paying for.<\/div>\n<div class=\"faq\">\n<h3>Why does polycarbonate sheet yellow?<\/h3>\n<p>Oxidation at melt temperature produces coloured species. It is cumulative with time and temperature, and it roughly doubles for every twenty degrees.<\/p>\n<h3>What melt temperature should PC run at?<\/h3>\n<p>280 to 310 C. Above about 310 the yellowness index passes 3, which is where a clear sheet starts to read as warm.<\/p>\n<h3>How long does PC need to dry?<\/h3>\n<p>Three to four hours at 120 C to reach 200 ppm. At 100 C it takes eight hours, and at 130 C two, but 130 is close to the sticking range.<\/p>\n<h3>Why is the cut edge amber?<\/h3>\n<p>You are looking through the full thickness rather than the face, so the polymer's intrinsic absorption is multiplied. It is geometry, not contamination.<\/p>\n<h3>Can yellow sheet be fixed by lowering the temperature?<\/h3>\n<p>Only if the residence time is normal. If the barrel is oversized for the shot, the material is degrading for eight minutes and no setpoint will fix it.<\/p>\n<h3>What is the invisible failure mode?<\/h3>\n<p>Hydrolysis. The sheet stays clear and loses impact strength, so it passes every visual check and fails on the first impact.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Sheet that has to stay clear and stay tough?<\/p>\n<p>Send the thickness, the forming temperature and the impact requirement. We will tell you what the drying schedule and melt window have to be to hold both.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ko\/%ed%94%8c%eb%9d%bc%ec%8a%a4%ed%8b%b1-%ec%95%95%ec%b6%9c-%ec%86%94%eb%a3%a8%ec%85%98\/\">Ask about polycarbonate sheet<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ko\/pet-sheet-extrusion\/\">PET Sheet Extrusion: Water Is Measured in Parts per Million<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ko\/pvc-foam-board-extrusion\/\">PVC Foam Board: The Lightest Sheet Is the Worst Insulator<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ko\/thermoforming-tolerances\/\">Thermoforming Tolerances: What a Formed Part Can Hold<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ko\/profile-cnc-fabrication\/\">Profile CNC Fabrication: Cutting Without Changing the Face<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ko\/%ed%94%8c%eb%9d%bc%ec%8a%a4%ed%8b%b1-%ec%95%95%ec%b6%9c-%ec%86%94%eb%a3%a8%ec%85%98\/\">Plastic Extrusion Solutions: Process, Tolerance and Material<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Yellowness index runs 1.2 at 280 C and 14 at 360 C, so twenty degrees roughly doubles it. Drying takes eight hours at 100 C and two at 130 C, and the same moisture that hydrolyses the chain also leaves the sheet hazy.<\/p>","protected":false},"author":1,"featured_media":8044,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[17],"tags":[],"class_list":["post-8047","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-plastic-extrusion-process"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/posts\/8047","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/comments?post=8047"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/posts\/8047\/revisions"}],"predecessor-version":[{"id":8684,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/posts\/8047\/revisions\/8684"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/media\/8044"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/media?parent=8047"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/categories?post=8047"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/tags?post=8047"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}