{"id":7800,"date":"2025-10-09T09:00:00","date_gmt":"2025-10-09T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/hdpe-thermoforming\/"},"modified":"2026-10-28T09:22:29","modified_gmt":"2026-10-28T09:22:29","slug":"hdpe-thermoforming","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ko\/hdpe-thermoforming\/","title":{"rendered":"HDPE Thermoforming: A 20 \u00b0C Window, Heavy Sag and Shrinkage That Continues After Demoulding"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/hdpe-thermoforming.jpg\" alt=\"HDPE thermoforming window by thickness and post-forming shrinkage over 24 hours\" width=\"1536\" height=\"909\"><figcaption>Eighty percent of the shrinkage happens in the first four hours. Measure the part tomorrow.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"difficult\">Why HDPE is the awkward one<\/h2>\n<p>Polyethylene is the largest thermoforming material by volume, and almost all of that volume is thin-gauge packaging where the sheet is 0.3 to 1.0 mm and the part is shallow. Move to thick-gauge forming of HDPE and the material becomes difficult quickly.<\/p>\n<p>Three properties cause it. HDPE is semi-crystalline with a sharp melting range, so it goes from stiff to sagging over about 15 \u00b0C rather than softening gradually. It has low melt strength, so a hot sheet will not support its own weight. And it shrinks 1.5 to 2.8 percent on cooling, which continues after the part leaves the mould.<\/p>\n<p>The result is a material that forms well in a narrow band and badly everywhere else, and a part that changes size after it has been measured.<\/p>\n<table>\n<thead>\n<tr>\n<th>Grade<\/th>\n<th>\ubc00\ub3c4<\/th>\n<th>Forming note<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>LDPE<\/td>\n<td>0.92 g\/cm\u00b3<\/td>\n<td>Softest, sags most, lowest stiffness<\/td>\n<\/tr>\n<tr>\n<td>LLDPE<\/td>\n<td>0.92 \u2013 0.94 g\/cm\u00b3<\/td>\n<td>Tougher, better melt strength<\/td>\n<\/tr>\n<tr>\n<td>HDPE<\/td>\n<td>0.94 \u2013 0.96 g\/cm\u00b3<\/td>\n<td>Stiffest, narrowest window<\/td>\n<\/tr>\n<tr>\n<td>HMW-HDPE<\/td>\n<td>0.94 \u2013 0.96 g\/cm\u00b3<\/td>\n<td>Best melt strength, hardest to form<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 Polyethylene grades for thermoforming. Higher density means more stiffness and less forgiveness.<\/p>\n<h2 id=\"window\">The 20 \u00b0C window<\/h2>\n<p>HDPE forms between 138 and 172 \u00b0C at the surface, and the practical band for thick-gauge work is 145 to 165 \u00b0C. Below 145 the sheet is stiff and springs back after demoulding. Above 165 it sags so much that the geometry has changed before the mould arrives.<\/p>\n<p>The window narrows as the sheet gets thicker, because a thick sheet has a larger thermal gradient and the surface reaches forming temperature while the core is still cold. A 6 mm HDPE sheet needs a long soak at moderate temperature rather than a short burst at high temperature.<\/p>\n<p>Two-sided heating is essential. HDPE has low thermal conductivity, and a single-sided oven produces a sheet whose hot face is at 165 \u00b0C and whose cold face is at 130. The hot face sags and the cold face resists, and the part that results has a wall thickness gradient that follows the temperature gradient.<\/p>\n<table>\n<thead>\n<tr>\n<th>\ub450\uaed8<\/th>\n<th>Surface temperature<\/th>\n<th>\ub09c\ubc29 \uc2dc\uac04<\/th>\n<th>Mould temperature<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>2 mm<\/td>\n<td>145 \u2013 160 \u00b0C<\/td>\n<td>40 \u2013 60 s<\/td>\n<td>40 \u2013 60 \u00b0C<\/td>\n<\/tr>\n<tr>\n<td>3 mm<\/td>\n<td>148 \u2013 165 \u00b0C<\/td>\n<td>70 \u2013 100 s<\/td>\n<td>45 \u2013 65 \u00b0C<\/td>\n<\/tr>\n<tr>\n<td>5 mm<\/td>\n<td>150 \u2013 168 \u00b0C<\/td>\n<td>130 \u2013 180 s<\/td>\n<td>50 \u2013 70 \u00b0C<\/td>\n<\/tr>\n<tr>\n<td>8 mm<\/td>\n<td>152 \u2013 170 \u00b0C<\/td>\n<td>230 \u2013 310 s<\/td>\n<td>55 \u2013 75 \u00b0C<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 HDPE thick-gauge forming parameters. Mould temperature is higher than for thin-gauge work because it controls shrinkage as well as surface.<\/p>\n<h2 id=\"sag\">Sag and webbing<\/h2>\n<p>HDPE sags more than any other common thermoforming material at the same temperature relative to its melting point. A 3 mm sheet at 160 \u00b0C will sag 40 to 60 mm across a 600 mm span, and once it has sagged the sheet is no longer uniformly hot.<\/p>\n<p>Webbing follows from sag. Where the sheet has sagged between two deep features, the material there is thinner and hotter, so it stretches first and folds onto itself. The fold cools into a permanent crease that cannot be removed and usually has to be trimmed out.<\/p>\n<p>Three levers control it, in order of effectiveness. Reduce the unsupported span by using a plug or a billow. Profile the heaters so the web region is cooler. Reduce the overall temperature and accept a slower cycle. Reducing temperature alone produces a part that does not form, which is why it is the last resort.<\/p>\n<div class=\"callout\">Billow forming \u2014 pre-stretching the sheet with air pressure before it touches the mould \u2014 is the standard answer for deep HDPE parts. It uses the sheet's own low melt strength against itself.<\/div>\n<h2 id=\"shrink\">Shrinkage that continues after demoulding<\/h2>\n<p>A formed HDPE part shrinks 1.5 to 2.8 percent in the first 24 hours, and about 80 percent of that happens in the first four. A part measured immediately after demoulding is larger than the part that ships.<\/p>\n<p>The shrinkage is anisotropic and follows the draw direction. Material that was stretched along the draw shrinks more when it relaxes, so a deep part is shorter in the draw direction than across it by 0.3 to 0.6 percentage points.<\/p>\n<p>The mould must be cut oversize to compensate, and the compensation is specific to the material, the draw ratio and the cooling. A tool cut for 2 percent will produce parts that are right at one draw ratio and wrong at another. Where a part has features at different draw depths, no single shrinkage factor is correct and the design must allow for it.<\/p>\n<p>The practical answer is to measure. Form three parts, measure them at 1 hour, 4 hours and 24 hours, and cut the tool from the 24-hour numbers. A toolmaker who asks for a shrinkage figure should be given three numbers with the measurement times attached.<\/p>\n<h2 id=\"mould\">Moulds and cooling<\/h2>\n<p>HDPE moulds are aluminium for most work. Mould temperature is 40 to 75 \u00b0C, warmer than for thin-gauge work because a warm mould reduces the thermal shock that produces frozen stress and post-mould distortion.<\/p>\n<p>Cooling must be uniform. HDPE has a high heat of crystallisation, so a thick section releases heat as it crystallises and a mould that removes heat unevenly produces differential crystallinity and therefore differential shrinkage. The part warps in the direction of the cooler region.<\/p>\n<p>Vacuum holes must be large enough. HDPE at forming temperature is viscous and will bridge over a 0.5 mm hole without pulling into it, leaving a dimple or an unformed area. Holes of 0.8 to 1.2 mm at 25 mm spacing are typical for thick-gauge HDPE.<\/p>\n<h2 id=\"defects\">Defects<\/h2>\n<table>\n<thead>\n<tr>\n<th>\uacb0\ud568<\/th>\n<th>\uc6d0\uc778<\/th>\n<th>Fix<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Webbing between features<\/td>\n<td>Sag and hot web region<\/td>\n<td>Billow or plug, profile the heaters<\/td>\n<\/tr>\n<tr>\n<td>Spring-back after demould<\/td>\n<td>Sheet too cold<\/td>\n<td>Raise 8 \u00b0C, increase soak time<\/td>\n<\/tr>\n<tr>\n<td>Warp after 24 hours<\/td>\n<td>Differential crystallinity<\/td>\n<td>Even mould temperature, slower cooling<\/td>\n<\/tr>\n<tr>\n<td>Unformed corners<\/td>\n<td>Vacuum holes too small or blocked<\/td>\n<td>Enlarge and clean the holes<\/td>\n<\/tr>\n<tr>\n<td>Thin base<\/td>\n<td>Excessive draw ratio<\/td>\n<td>Reduce depth or add plug assist<\/td>\n<\/tr>\n<tr>\n<td>Part sticks<\/td>\n<td>Insufficient draft<\/td>\n<td>Add 2 \u2013 3\u00b0 draft<\/td>\n<\/tr>\n<tr>\n<td>Surface orange peel<\/td>\n<td>Mould too cold or vacuum too fast<\/td>\n<td>Warm the mould, slow the vacuum<\/td>\n<\/tr>\n<tr>\n<td>Dimensional drift<\/td>\n<td>Shrinkage not allowed for<\/td>\n<td>Measure at 24 h and re-cut<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 \u2014 HDPE thermoforming defects. Two of them are consequences of the material's crystallinity, which is why they are not fixable by tuning alone.<\/p>\n<div class=\"faq\">\n<h3>What is the forming temperature for HDPE sheet?<\/h3>\n<p>138 to 172 \u00b0C at the surface, with 145 to 165 \u00b0C the practical band for thick-gauge work. Below 145 the sheet springs back; above 165 it sags beyond control.<\/p>\n<h3>How much does a thermoformed HDPE part shrink?<\/h3>\n<p>1.5 to 2.8 percent in the first 24 hours, with about 80 percent in the first four hours. Measure at 24 hours and cut the tool from those numbers.<\/p>\n<h3>Why does HDPE web so badly?<\/h3>\n<p>Low melt strength and a narrow forming window. The sheet sags between features, the web region gets thinner and hotter, and it folds. Billow forming or a plug is the usual fix.<\/p>\n<h3>Can HDPE be thermoformed without a plug?<\/h3>\n<p>For shallow parts, yes. Above a draw ratio of about 0.6, a plug or billow is needed to control the wall distribution and prevent webbing.<\/p>\n<h3>What mould temperature for HDPE thermoforming?<\/h3>\n<p>40 to 75 \u00b0C, warmer for thicker sheet. A warm mould reduces frozen stress and the post-mould distortion that follows it.<\/p>\n<h3>Why does my HDPE part change size overnight?<\/h3>\n<p>Crystallisation continues after demoulding. The part is still organising its structure for several hours. Allow for it in the tool and measure the part the next day, not the same shift.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Forming thick-gauge HDPE parts?<\/p>\n<p>Send us the drawing, the wall and the draw depth. We will tell you whether the part needs billow forming and what shrinkage to cut for.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ko\/custom-vacuum-forming\/\">Talk to a thermoforming engineer<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ko\/hdpe-injection-molding\/\">HDPE Injection Molding: Shrinkage and Settings<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ko\/hdpe-pipe-extrusion\/\">HDPE Pipe Extrusion: Sag, Ovality and Cooling<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ko\/pp-thin-gauge-thermoforming\/\">PP Thin Gauge Thermoforming<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ko\/thermoforming-sheet-heating-temperature-window\/\">Thermoforming Sheet Heating Temperature Window<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ko\/vacuum-forming-wall-thickness\/\">Thermoforming Wall Thickness<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>HDPE is cheap, tough and chemically resistant, and it is the most awkward polyolefin to thermoform. The window is 20 \u00b0C, the sheet sags, and the part keeps shrinking for a day.<\/p>","protected":false},"author":1,"featured_media":7799,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[29],"tags":[],"class_list":["post-7800","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-vacuum-forming"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/posts\/7800","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/comments?post=7800"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/posts\/7800\/revisions"}],"predecessor-version":[{"id":7864,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/posts\/7800\/revisions\/7864"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/media\/7799"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/media?parent=7800"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/categories?post=7800"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ko\/wp-json\/wp\/v2\/tags?post=7800"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}