{"id":7491,"date":"2026-10-25T10:44:33","date_gmt":"2026-10-25T10:44:33","guid":{"rendered":"https:\/\/uplastech.com\/plastic-extrusion-defects\/"},"modified":"2026-10-26T07:41:59","modified_gmt":"2026-10-26T07:41:59","slug":"%e3%83%97%e3%83%a9%e3%82%b9%e3%83%81%e3%83%83%e3%82%af%e6%8a%bc%e5%87%ba%e4%b8%8d%e8%89%af","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ja\/%e3%83%97%e3%83%a9%e3%82%b9%e3%83%81%e3%83%83%e3%82%af%e6%8a%bc%e5%87%ba%e4%b8%8d%e8%89%af\/","title":{"rendered":"Plastic Extrusion Defects: 12 Problems, Causes and Fixes"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u81ea\u52a8\u5c55\u5f00\u7684\u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2024\/11\/Plastic-Extrusion-Molds.jpg\" alt=\"Machined steel extrusion die plates used for plastic profile production\" width=\"700\" height=\"900\"><figcaption>Half the defects in this guide are decided inside the die, not on the control panel. Knowing which half saves days of parameter chasing.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"diagnose\">Diagnose before you adjust<\/h2>\n<p>Extrusion is a continuous process, so a defect that appears at one point on the line will repeat on every metre after it. That makes diagnosis easier than in injection moulding \u2014 you can see exactly where in the line the problem starts, and you can watch it change as you adjust one variable.<\/p>\n<p>Three questions identify most extrusion defects before any setting is touched:<\/p>\n<ul>\n<li><strong>Does it appear before or after the calibration sleeve?<\/strong> A defect visible at the die but gone after calibration is a die or melt problem. A defect that appears only after calibration is a cooling, vacuum or haul-off problem. This single observation halves the search.<\/li>\n<li><strong>Does it change with line speed?<\/strong> If the defect worsens when you speed up, it is shear or cooling related. If it is unaffected by speed, it is usually tooling or material.<\/li>\n<li><strong>Is it continuous, periodic or random?<\/strong> Continuous means a steady-state cause \u2014 die condition, temperature, formulation. Periodic points at something rotating: a screw, a haul-off belt, a worn idler, a gear pump. Random points at contamination or feed variation.<\/li>\n<\/ul>\n<div class=\"callout\">\n<p><strong>The order that wastes least time:<\/strong> material and drying \u2192 die condition (clean, no damage, no build-up) \u2192 melt temperature profile \u2192 screw speed and output \u2192 calibration vacuum and water temperature \u2192 haul-off and take-up tension. Most people start at the haul-off and work backwards.<\/p>\n<\/div>\n<h2 id=\"dimension\">Out-of-tolerance cross-section<\/h2>\n<p>The profile is the right shape but the wrong size \u2014 a wall too thick, an outside dimension drifting, a chamber collapsing slightly. This is the most common extrusion complaint and the most expensive, because it usually means scrap that has already been coiled or bundled.<\/p>\n<p><strong>Causes.<\/strong> Die wear in the land area, which increases flow and thickens the wall. A worn or scored calibration sleeve, which no longer holds the outside dimension. Melt temperature drift, which changes both viscosity and drawdown. Haul-off speed drifting relative to extruder output, which changes the drawdown ratio. Vacuum loss in the calibration tank. A formulation change \u2014 a different filler loading or a different regrind ratio changes shrinkage and drawdown.<\/p>\n<p><strong>Fixes.<\/strong> First check the calibration vacuum and the water temperature, because they are the cheapest to verify. Then measure the haul-off speed and the screw speed together and confirm the drawdown ratio is what it was at first-article approval. Then check the die and sleeve for wear with a pin gauge \u2014 a sleeve worn by 0.1 mm shows up as a 0.1 mm dimension shift, which is enough to fail a tight tolerance.<\/p>\n<p><strong>The pattern to watch.<\/strong> A dimension that drifts slowly over days is wear. A dimension that jumps between shifts is a setting or a different operator. A dimension that changes with the season is usually cooling water temperature.<\/p>\n<h2 id=\"melt-fracture\">Melt fracture and sharkskin<\/h2>\n<p>A fine, regular, matte ripple across the surface \u2014 sometimes called sharkskin \u2014 or in severe cases a rough, torn, spiral surface. It appears when the surface shear stress at the die exit exceeds what the melt can withstand.<\/p>\n<p><strong>Causes.<\/strong> Output too high for the die land length. Melt temperature too low, raising viscosity. A die land that is too short, so the melt does not have time to relax before exiting. A die lip that is damaged or poorly polished. A material with a very high molecular weight or a high filler loading, which fractures at lower shear rates.<\/p>\n<p><strong>Fixes.<\/strong> Raise the melt temperature in 5 \u00b0C steps \u2014 this is the fastest fix and usually enough. Reduce output. If the problem returns at the required output, the die needs a longer land or a larger die opening, which is a tool modification. A fluoropolymer processing aid can raise the critical shear rate significantly and is a legitimate formulation fix for a difficult section.<\/p>\n<p><strong>Do not<\/strong> try to polish out sharkskin. It is not a surface defect; it is a flow instability that happens <em>after<\/em> the melt leaves the die. Polishing the lip will not remove it.<\/p>\n<h2 id=\"die-lines\">Die lines and drag lines<\/h2>\n<p>Continuous longitudinal lines running the length of the profile, usually straight and often on one face. They are the easiest defect to diagnose because their position on the section points directly at the location on the die.<\/p>\n<p><strong>Causes.<\/strong> A scratch or nick on the die land or the die lip. Carbonised material or additive build-up (plate-out) on the die. A burr on the calibration sleeve entry. Poor die polishing in a corner or a narrow channel. In PVC, a build-up of degraded material at a flow stagnation point.<\/p>\n<p><strong>Fixes.<\/strong> Locate the line on the section, then inspect the die at the corresponding angular position. Clean and polish. If the line returns within hours, the cause is build-up rather than damage, and the fix is a formulation or die-temperature adjustment \u2014 a slightly hotter die land reduces adhesion of the deposit.<\/p>\n<p><strong>Why it matters commercially.<\/strong> A die line on a hidden face is cosmetic and may be acceptable. The same line on a visible face fails first-article approval and, if it reaches the customer, generates a return. Agree which faces are cosmetic before the tool is cut.<\/p>\n<h2 id=\"bubbles\">Bubbles and voids<\/h2>\n<p>Bubbles visible through a translucent profile, or blisters on the surface. In an opaque profile they may only show up when the part is cut or when a section is x-rayed.<\/p>\n<p><strong>Causes.<\/strong> Moisture in the resin, which turns to steam in the barrel. Air entrained at the feed throat because the feed is too hot or the screw is starving. Volatiles from an overheated melt or from a high regrind content. A vent that is blocked, on a vented extruder. Decomposition of a blowing agent where one is not wanted \u2014 a risk when cellular and rigid PVC run on the same line.<\/p>\n<p><strong>Fixes.<\/strong> Dry the material and verify the dryer rather than trusting it. Check the feed throat temperature \u2014 a hot feed throat causes the pellets to stick and the screw to starve, drawing air. Reduce melt temperature. Check the vent. Reduce the regrind ratio and confirm the regrind is dry.<\/p>\n<p><strong>The distinguishing test.<\/strong> Cut the profile and look at the bubbles. Moisture bubbles are round, evenly distributed and often concentrated toward the centre. Air entrainment gives elongated voids aligned with the flow. Volatile bubbles are irregular and usually accompanied by a smell.<\/p>\n<h2 id=\"specks\">Black specks and carbon<\/h2>\n<p>Dark particles embedded in an otherwise good profile, ranging from a few microns to several millimetres. In a white profile they are immediately visible and are an automatic reject.<\/p>\n<p><strong>Causes.<\/strong> Degraded material held in a dead spot \u2014 behind the screw flight, in a breaker plate, in a screen pack, in a die channel that is not swept by flow. Overheated zones producing local degradation. A worn screw or barrel with excessive clearance. Contaminated regrind or a dirty feed system. In PVC, any period of stopped flow.<\/p>\n<p><strong>Fixes.<\/strong> Purge with a proper purging compound rather than with virgin resin, and change the screen pack. Check every zone against the temperature profile. If the specks return within a shift, the problem is a dead spot in the flow path and the screw or die has to come out.<\/p>\n<p><strong>The preventive discipline.<\/strong> Black specks are almost always a shutdown-and-startup problem, not a running problem. A documented purge procedure at every stop, and a barrel kept at temperature with the screw forward during short stops, prevents most of them.<\/p>\n<h2 id=\"roughness\">Rough surface, orange peel, poor gloss<\/h2>\n<p>A general loss of gloss, a stippled or pebbled surface, or a mottled appearance. Different from melt fracture, which is a regular high-frequency ripple.<\/p>\n<p><strong>Causes.<\/strong> Melt temperature too low, so the compound does not fuse properly against the die and the calibrator. Moisture. A die land that is too short or too cold. Insufficient vacuum in the calibration sleeve, so the surface is not pressed against the polished sleeve. A calibration sleeve that is contaminated or has lost its polish. Too much filler or an incompatible additive in the formulation.<\/p>\n<p><strong>Fixes.<\/strong> Raise the melt and die temperature. Check the vacuum level at the sleeve \u2014 a leaking seal or a blocked vacuum slot reduces it. Clean and polish the sleeve. If the surface is mottled rather than uniformly rough, the cause is mixing and the answer is a screw or formulation change.<\/p>\n<h2 id=\"warpage\">Warpage and bend<\/h2>\n<p>The profile is dimensionally correct on the line and bends, twists or cups after cooling, or after a day in the warehouse.<\/p>\n<p><strong>Causes.<\/strong> Differential cooling \u2014 one side of the profile cooling faster than the other, usually because the water is directed at one face. Uneven wall thickness, so thick sections are still shrinking when thin ones have frozen. Asymmetric section design, where the mass is not balanced about the centreline. Too-rapid cooling overall, which locks in stress. Haul-off or take-up tension applied while the profile is still soft. Improper stacking or coiling while warm.<\/p>\n<p><strong>Fixes.<\/strong> Balance the cooling first \u2014 check that water is distributed around the whole section and that both sides of a flat profile see the same temperature. Slow the cooling slightly and lengthen the tank. Reduce haul-off tension. Allow the profile to cool before it is bundled or coiled.<\/p>\n<p><strong>The design point.<\/strong> An asymmetric section will always want to bend, and no amount of process tuning fully removes it. A cooling fixture or a short annealing pass after the tank is often the practical answer, and a balanced section is the permanent one.<\/p>\n<h2 id=\"sink\">Sink marks in thick walls<\/h2>\n<p>A depression on the surface opposite a thick section or a heavy rib. Less common in extrusion than in injection moulding, because the melt is under continuous pressure, but it appears wherever the wall is thick enough to shrink after the skin has frozen.<\/p>\n<p><strong>Causes.<\/strong> A wall section that is too thick for the cooling available. Insufficient melt pressure at the die, so the section is not packed. Vacuum pulling a soft wall inward. A hollow chamber with too little internal support pressure. Too-fast cooling on the outside relative to the inside.<\/p>\n<p><strong>Fixes.<\/strong> Reduce the wall thickness \u2014 this is the real answer and it is a design change. Raise the internal pressure on a hollow profile. Adjust the vacuum so it holds the outer surface without collapsing the wall. Slow the cooling on the thick side.<\/p>\n<h2 id=\"colour\">Colour streaks and shade variation<\/h2>\n<p>Swirls, dark streaks, light patches, or a shade that drifts over the length of a run.<\/p>\n<p><strong>Causes.<\/strong> Masterbatch or pigment not dispersed, because the melt temperature is low or the screw has insufficient mixing. A let-down ratio that is wrong or inconsistent. Screw wear producing unmelted particles. Dead spots in the die holding degraded material. Regrind ratio varying through the run. For a pre-compounded colour, a batch-to-batch difference from the compounder.<\/p>\n<p><strong>Fixes.<\/strong> Raise back pressure and melt temperature to improve dispersion. Verify the let-down ratio by weighing. Fix the regrind ratio and hold it constant rather than topping up with whatever is available. If the shade drifts gradually over hours, the cause is usually thermal \u2014 the die is slowly building up or the compound is slowly changing.<\/p>\n<p><strong>The commercial detail.<\/strong> Colour is judged against a standard under a specified light source. Agree the standard, the light source and the acceptable colour difference before the first run, otherwise every shipment becomes a negotiation.<\/p>\n<h2 id=\"delam\">Delamination<\/h2>\n<p>The outer layer separates from the core \u2014 in a co-extruded profile, a laminated profile, or a profile made from mixed regrind. It shows as a peeling edge, a blister along the length, or a layer that can be lifted with a fingernail.<\/p>\n<p><strong>Causes.<\/strong> Incompatible materials at the interface. Interface temperature too low, so the two melts do not entangle before freezing. Contamination \u2014 moisture, oil or dust \u2014 at the interface. A co-extrusion die that is not bringing the streams together at the right point. In a laminated profile, an adhesive that is under-cured or applied too thin. In mixed regrind, incompatible polymer contamination.<\/p>\n<p><strong>Fixes.<\/strong> Raise the interface temperature by adjusting the two melt temperatures toward each other. Confirm the material pairing against a compatibility chart rather than assuming. Clean the die and the feed system. For laminated profiles, check the adhesive and the laminating roll temperature.<\/p>\n<p><strong>The one that cannot be fixed on the line.<\/strong> If the two polymers are chemically incompatible, no setting will produce a bond. That is a design decision that has to be reversed, not a process problem.<\/p>\n<h2 id=\"cracks\">Cracks after cutting<\/h2>\n<p>The profile is sound on the line, then cracks at the cut end, along a corner, or between chambers \u2014 sometimes minutes later, sometimes days later.<\/p>\n<p><strong>Causes.<\/strong> Internal stress from too-rapid cooling, released when the profile is cut. A dull or misaligned saw blade, which introduces a notch. Cutting the profile while it is still warm. A sharp internal corner acting as a stress concentrator. In PVC, a formulation with insufficient impact modifier. Solvent contact after extrusion \u2014 some cleaning agents will stress-craze PVC and polycarbonate.<\/p>\n<p><strong>Fixes.<\/strong> Slow the cooling so the profile leaves the tank closer to ambient. Sharpen and align the blade, and check the cut-off saw's clamp pressure. Cut cool rather than warm. Increase the corner radii on the section.<\/p>\n<p><strong>Why it is worth chasing.<\/strong> A crack that appears after delivery looks like a material failure and destroys confidence in the whole shipment, even when the root cause is a saw blade. If cracks appear after a delay, an annealing pass is the usual remedy while the process is corrected.<\/p>\n<h2 id=\"cut\">Cut length and cut angle<\/h2>\n<p>Lengths outside tolerance, ends not square, or a length that varies within a bundle.<\/p>\n<p><strong>Causes.<\/strong> Haul-off speed varying, or the encoder slipping on the profile. A cut-off saw that is not synchronized with the haul-off. Blade deflection on a large section. The profile moving during the cut because the clamp is worn. Thermal expansion \u2014 a profile cut warm and measured cold will be short.<\/p>\n<p><strong>Fixes.<\/strong> Check the encoder wheel for wear and slip, and confirm it is running on a clean, dry surface. Verify the saw is synchronized rather than free-running. Replace worn clamp pads. For tight length tolerances, measure at a defined temperature and state it in the specification.<\/p>\n<h2 id=\"matrix\">The troubleshooting matrix<\/h2>\n<p>Read across, not down. A defect with a plausible cause in only one column is usually that cause.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u6b20\u9665<\/th>\n<th>Process &amp; screw<\/th>\n<th>Die &amp; tooling<\/th>\n<th>Cooling, calibration, haul-off<\/th>\n<th>\u7d20\u6750<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td><strong>Out of tolerance<\/strong><\/td>\n<td>Melt temp drift, output<\/td>\n<td>Die or sleeve wear<\/td>\n<td>Vacuum loss, drawdown ratio<\/td>\n<td>Formulation, regrind ratio<\/td>\n<\/tr>\n<tr>\n<td><strong>Melt fracture<\/strong><\/td>\n<td>Output too high, temp too low<\/td>\n<td>Land too short, lip damaged<\/td>\n<td>\u2014<\/td>\n<td>High viscosity, high filler<\/td>\n<\/tr>\n<tr>\n<td><strong>Die lines<\/strong><\/td>\n<td>Die temperature<\/td>\n<td>Scratch, build-up, poor polish<\/td>\n<td>Sleeve burr<\/td>\n<td>Plate-out from additives<\/td>\n<\/tr>\n<tr>\n<td><strong>Bubbles<\/strong><\/td>\n<td>Feed throat heat, venting<\/td>\n<td>Blocked vent<\/td>\n<td>\u2014<\/td>\n<td>Moisture, volatiles, regrind<\/td>\n<\/tr>\n<tr>\n<td><strong>Black specks<\/strong><\/td>\n<td>Dead spots, overheating<\/td>\n<td>Unswept die channel<\/td>\n<td>\u2014<\/td>\n<td>Contamination, degraded regrind<\/td>\n<\/tr>\n<tr>\n<td><strong>Rough surface<\/strong><\/td>\n<td>Melt temp too low<\/td>\n<td>Land too short or cold<\/td>\n<td>Low vacuum, dirty sleeve<\/td>\n<td>Moisture, excess filler<\/td>\n<\/tr>\n<tr>\n<td><strong>\u53cd\u308a<\/strong><\/td>\n<td>\u2014<\/td>\n<td>Unbalanced section<\/td>\n<td>Uneven cooling, haul-off tension<\/td>\n<td>High shrinkage, anisotropic filler<\/td>\n<\/tr>\n<tr>\n<td><strong>Sink<\/strong><\/td>\n<td>Melt pressure<\/td>\n<td>Wall too thick<\/td>\n<td>Vacuum too high<\/td>\n<td>High shrinkage<\/td>\n<\/tr>\n<tr>\n<td><strong>Colour streaks<\/strong><\/td>\n<td>Mixing, back pressure<\/td>\n<td>Die dead spots<\/td>\n<td>\u2014<\/td>\n<td>Dispersion, let-down, regrind<\/td>\n<\/tr>\n<tr>\n<td><strong>Delamination<\/strong><\/td>\n<td>Interface temperature<\/td>\n<td>Streams meet too early<\/td>\n<td>\u2014<\/td>\n<td>Incompatible pair, contamination<\/td>\n<\/tr>\n<tr>\n<td><strong>Cracks after cut<\/strong><\/td>\n<td>Cooling rate<\/td>\n<td>Sharp corners<\/td>\n<td>Blade condition, cut temperature<\/td>\n<td>Impact modifier level<\/td>\n<\/tr>\n<tr>\n<td><strong>Cut length<\/strong><\/td>\n<td>\u2014<\/td>\n<td>\u2014<\/td>\n<td>Encoder slip, saw sync, clamp wear<\/td>\n<td>Thermal expansion<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Cooling, calibration and haul-off carry more defects in extrusion than in injection moulding, because a continuous process has no natural end point where the part is \"done\".<\/p>\n<h2 id=\"die-not-process\">When it is the die, not the process<\/h2>\n<p>Some defects cannot be processed out. Recognising them early saves weeks of parameter chasing.<\/p>\n<ul>\n<li><strong>The defect is in the same angular position on the section every time.<\/strong> That is a specific location on the die or the sleeve.<\/li>\n<li><strong>The defect survives a full die clean and a new screen pack.<\/strong> It is damage or a design problem, not contamination.<\/li>\n<li><strong>The defect appears at every output and every temperature.<\/strong> The die geometry is wrong for the section.<\/li>\n<li><strong>One face is rough and the opposite face is fine.<\/strong> Asymmetric flow in the die.<\/li>\n<li><strong>The profile is out of tolerance in a way that no drawdown adjustment fixes.<\/strong> The die was cut to the wrong allowance.<\/li>\n<li><strong>The defect only appears above a certain line speed and never goes away.<\/strong> The die land is too short for the output the commercial case requires.<\/li>\n<\/ul>\n<p>The commercial point: a defect that needs a die modification should be found during first-article approval, on a few hundred metres, not after twenty thousand metres have been coiled. That is what a proper first-article dimensional report and a retained sample are for.<\/p>\n<h2 id=\"faq\">Frequently asked questions<\/h2>\n<div class=\"faq\">\n<h3>What is the most common extrusion defect?<\/h3>\n<p>Out-of-tolerance cross-section, and it is usually traced to the calibration sleeve rather than the die. The sleeve sets the outside dimension, it wears, and it is often the last thing anyone checks. Die lines are second, and are the easiest to diagnose because the position of the line points directly at the location on the die.<\/p>\n<h3>Why does my profile only warp in summer?<\/h3>\n<p>Cooling water temperature. In summer the plant water is warmer, the cooling rate drops, and a profile that was balanced at 15 \u00b0C water is no longer balanced at 25 \u00b0C. The other seasonal factor is ambient temperature affecting how the profile cools after the tank. Chilled water and a controlled plant temperature remove both effects.<\/p>\n<h3>How do I tell melt fracture from a dirty die?<\/h3>\n<p>Melt fracture is a regular, high-frequency ripple that covers the whole surface and changes when you change output or temperature. A dirty die or a die line is a distinct longitudinal line at one position. If the defect responds to output, it is melt fracture; if it stays in the same place regardless, it is the die.<\/p>\n<h3>Can black specks be prevented without stopping the line?<\/h3>\n<p>Not reliably. Black specks come from degraded material in dead spots, and the only real fix is to purge and clean. What can be prevented is the degradation itself: purge at every stop, keep the barrel at temperature with the screw forward during short stops, and change the screen pack on a schedule rather than when specks appear.<\/p>\n<h3>Is it normal for a new die to need several trials?<\/h3>\n<p>Yes. Two or three trials is normal for a profile with hollow chambers or tight tolerances, because the drawdown allowance and the flow balance have to be corrected against real output. What is not normal is a die that produces a different defect after every trial without the die being changed \u2014 that pattern means the process is being used to compensate for a tool problem.<\/p>\n<h3>Can you match a profile we already buy elsewhere?<\/h3>\n<p>Yes. Send a sample and the drawing. We measure the sample, identify the compound or a close equivalent, and cut the die against the measured section rather than the nominal drawing \u2014 which is usually the only way to make a replacement profile interchangeable with the original, especially where a sleeve has worn over the years.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Send us the defect \u2014 we will tell you where it comes from<\/p>\n<p>Photograph the profile with a scale alongside, tell us the material, the line speed and whether the defect appears before or after the calibration tank. We come back with the likely cause, the setting to change first, and whether the fix needs the die.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ja\/%e3%82%b5%e3%83%bc%e3%83%93%e3%82%b9\/\">Ask for a defect review<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ja\/co-extrusion-profiles\/\">Co-Extrusion Profiles: Dual Durometer, Tri-Extrusion and Bonding<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ja\/pvc-profile-extrusion\/\">PVC Profile Extrusion: Rigid, Flexible and Cellular PVC<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ja\/custom-plastic-extrusion-profiles-guide\/\">Custom Plastic Extrusion Profiles: Materials, Dies and Tolerances<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ja\/%e3%83%97%e3%83%a9%e3%82%b9%e3%83%81%e3%83%83%e3%82%af%e6%8a%bc%e5%87%ba%e3%82%bd%e3%83%aa%e3%83%a5%e3%83%bc%e3%82%b7%e3%83%a7%e3%83%b3\/\">Plastic extrusion solutions at Uplastech<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>A troubleshooting guide to the 12 most common plastic extrusion defects \u2014 out-of-tolerance section, melt fracture, die lines, bubbles, black specks, warpage, delamination and more \u2014 with causes, fixes and a four-column matrix.<\/p>","protected":false},"author":1,"featured_media":7250,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"_seopress_titles_title":"Plastic Extrusion Defects: 12 Problems, Causes and Fixes","_seopress_titles_desc":"Plastic extrusion defects explained: melt fracture, die lines, bubbles, black specks, warpage, sink, delamination, cracking \u2014 causes, fixes and a troubleshooting matrix.","_seopress_robots_index":"1","_seopress_robots_follow":"1","_seopress_robots_imageindex":"","_seopress_robots_snippet":"","_seopress_robots_primary_cat":"36","_seopress_robots_breadcrumbs":"","_seopress_robots_freeze_modified_date":"","_seopress_robots_custom_modified_date":"","_seopress_robots_canonical":"https:\/\/uplastech.com\/plastic-extrusion-defects\/","_seopress_social_fb_title":"","_seopress_social_fb_desc":"","_seopress_social_fb_img":"","_seopress_social_fb_img_attachment_id":0,"_seopress_social_fb_img_width":0,"_seopress_social_fb_img_height":0,"_seopress_social_twitter_title":"","_seopress_social_twitter_desc":"","_seopress_social_twitter_img":"","_seopress_social_twitter_img_attachment_id":0,"_seopress_social_twitter_img_width":0,"_seopress_social_twitter_img_height":0,"_seopress_redirections_value":"","_seopress_redirections_enabled":"","_seopress_redirections_enabled_regex":"","_seopress_redirections_logged_status":"","_seopress_redirections_param":"","_seopress_redirections_type":0,"_seopress_analysis_target_kw":"plastic extrusion defects","footnotes":""},"categories":[17,36],"tags":[],"class_list":["post-7491","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-plastic-extrusion-process","category-profile-extrusion"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/posts\/7491","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/comments?post=7491"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/posts\/7491\/revisions"}],"predecessor-version":[{"id":7550,"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/posts\/7491\/revisions\/7550"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/media\/7250"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/media?parent=7491"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/categories?post=7491"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ja\/wp-json\/wp\/v2\/tags?post=7491"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}