Cooling and Cycle Time in Vacuum Forming

Chart showing cooling time against sheet thickness in vacuum forming, with mould temperature as the parameter
Cooling is 45–70% of a thermoforming cycle, and it scales roughly with thickness squared. Everything else in the cycle is detail by comparison.

Where the cycle time actually goes

People new to thermoforming assume the forming step is the slow part. It is not. Forming takes two to ten seconds. Cooling takes two to four times as long, and it is the only part of the cycle that cannot be shortened by doing it faster.

Phase Share of cycle Typical time (2 mm sheet) Can it be shortened?
Load and clamp 5 – 10% 2 – 4 s Automazione
Riscaldamento 15 – 25% 8 – 15 s Better heaters, closer spacing
Forming (vacuum + draw) 3 – 8% 2 – 5 s Faster vacuum, more vent area
Cooling in the tool 50 – 70% 15 – 40 s Mould temperature, air assist
Demould and unload 5 – 10% 2 – 5 s Automazione

Table 1 — Cycle breakdown for thin gauge. On heavy gauge the cooling share climbs towards 70%: heat enters the sheet quickly but has to leave it through the thickness.

Cooling is the constraint because the part has to be stiff enough to demould without distorting. That is a material property, and the time to reach it is set by heat transfer — which follows a relationship you can calculate.

The relationship that governs everything

Cooling time in thermoforming follows the same square law as injection moulding: it scales with the square of the thickness. Double the sheet thickness and the cooling time roughly quadruples.

For a sheet cooled from both faces, the time to reach a given average temperature is approximately:

t ≈ (s² / (π² · α)) · ln( (8/π²) · (Tsheet − Tmould) / (Tdemould − Tmould) )

Where s is thickness, α is thermal diffusivity (about 0.10 mm²/s for most plastics), and the temperatures are sheet, mould and demould.

Sheet thickness Theoretical cooling Realistic with air assist Realistic without
0.5 mm 0.6 s 2 – 3 s 4 – 6 s
1.0 mm 1.4 s 4 – 6 s 8 – 12 s
2.0 mm 3.6 s 10 – 15 s 20 – 28 s
3.0 mm 7.0 s 18 – 26 s 35 – 45 s
4.0 mm 12 s 28 – 40 s 55 – 70 s
6.0 mm 26 s 55 – 80 s 110 – 140 s

Table 2 — Cooling time by sheet thickness. The gap between theory and practice is the tool interface: air gaps, contact quality and mould temperature control.

The gap between the theoretical and realistic numbers is where the money is. A 2 mm part that calculates at 3.6 s and runs at 25 s has 20 seconds of avoidable time in it — usually from poor contact between sheet and mould, or from a mould that is running too hot.

The four levers you actually have

Lever Effect Practical limit
Mould temperature Lower mould = faster cooling Below about 40 °C causes chill marks and stress
Air assist (blown air on the part) Adds convective cooling on the free face Needs a nozzle design that does not distort the part
Contact quality Vacuum holds the sheet against the tool Limited by part geometry and vent area
Demould temperature Eject sooner, at higher temperature Part must be stiff enough not to distort

Table 3 — The levers. Air assist is the biggest single gain available on an existing tool, and the cheapest to retrofit.

Air assist works by blowing ambient or chilled air onto the exposed face of the part while it is still on the tool. It roughly doubles the heat transfer coefficient on that face, which cuts cooling time by 25–40%. A simple manifold of nozzles is enough; it does not need to be a precision system.

The limit is distortion. Blowing air on a part that is still soft will push it out of shape, particularly on thin walls. The usual approach is to delay the air until the part has set enough to hold its shape, then blow hard.

Mould temperature: the quality constraint

Mould temperature Tempo di raffreddamento Part quality
20 – 30 °C (cold water) Fastest Chill marks, high stress, poor detail, possible distortion
40 – 60 °C Moderato Good balance for thin gauge
70 – 90 °C Lento Best surface detail, lowest stress
100 – 120 °C Slowest Needed for PC and heavy gauge; texture reproduction

Table 4 — Mould temperature trade-off. Running a cold mould to save cycle time costs surface quality and dimensional stability, which usually costs more downstream.

Cold moulds are the most common false economy in thermoforming. A mould at 25 °C will cut 30% off the cooling time and produce parts with chill marks, high residual stress and a surface that will not hold a texture. The customer sees the surface; nobody sees the cycle time.

Heavy gauge: where the cycle becomes a different problem

Above about 4 mm the cooling time dominates so completely that the process economics change. A 6 mm part might have a 90-second cooling time against a 30-second heating time, which means the machine is idle for two-thirds of the cycle unless it is designed for it.

Approccio How it works Effect
Accept the cycle Run slow, one part at a time Simple, but low output
Multiple tools on a carousel Several tools cycle through one heating station Machine runs continuously; capital cost
Twin-sheet or shuttle Two stations alternate Hides cooling behind heating
Cooling fixtures Part moves to a separate cooling jig Frees the tool for the next part

Table 5 — Handling long cooling times on heavy gauge. The carousel and the cooling fixture are the two that actually work; the rest just accept the loss.

The cooling fixture is the cheapest of these. The part comes off the tool while still warm and slightly flexible, is transferred to a shaped jig that holds it while it cools, and the tool is free for the next cycle. The jig costs a fraction of a second tool and it can cut effective cycle time by 40%.

Measuring and improving

Measurement How Target
Part surface temperature at demould IR gun or contact probe Below the resin's demould temperature
Mould surface temperature Probe at three points Uniform within 5 °C
Cooling water ΔT Inlet vs outlet Under 3 °C
Cycle time by phase Stopwatch or machine log Cooling under 65% of total
Distortion after 24 h Measure key dimensions Within tolerance

Table 6 — What to measure to improve the cycle. The water ΔT is the fastest diagnostic: a high ΔT means the mould is not transferring heat as designed.

Part temperature at demould is the number that tells you whether the cooling time is right. If the part comes off at 70 °C when the resin needs to be below 60 °C, it will distort after demould and the cycle is being pushed too hard. If it comes off at 45 °C, there is cooling time to give back.

How much of a vacuum forming cycle is cooling?

45–55% on thin gauge and around 70% on heavy gauge. It is the single largest phase and the only one that cannot be shortened by running faster — only by better heat transfer or a cooler mould.

Why does cooling time quadruple when thickness doubles?

Because heat has to conduct through the thickness, and conduction distance enters the equation squared. It is the same relationship as injection moulding, and it is why thick-gauge parts have such long cycles.

Does air assist really help?

Yes, 25–40% reduction in cooling time. Blowing air on the free face roughly doubles the heat transfer coefficient there. The constraint is distortion: the air has to be delayed until the part is stiff enough not to be pushed out of shape.

Can I run a colder mould to speed up the cycle?

You can, and you will get chill marks, high residual stress, poor surface detail and dimensional instability. Below about 40 °C the quality loss usually costs more than the cycle time saves. The exception is very thin, non-cosmetic parts.

How do I know when to demould?

Measure the part surface temperature. Every resin has a demould temperature below which it is stiff enough — typically 60–70 °C for PS and ABS, 80–90 °C for PP, 100–120 °C for PC. If it comes off hotter, it will distort.

What is the biggest cycle time mistake?

Setting cooling time by trial and error and then never revisiting it. Most machines run with 20–30% more cooling time than necessary because the setting was made once for a difficult part and never adjusted for easier ones.

Does the sheet thickness tolerance affect cycle time?

Yes. A sheet at the top of its thickness tolerance needs noticeably more cooling than one at the bottom, and if the cycle is set for the thin end, thick sheets will distort. Setting the cycle for the thickest sheet in the batch is the safe choice.

Is there a way to cool both sides?

On female tools with a male plug, the plug can be temperature controlled, which cools the inside. On simple vacuum forming there is only one tool face, which is why air assist exists — it is the only way to cool the free side.

Cycle time longer than it should be?

Send us the part drawing, material, gauge and current cycle breakdown. We will calculate what the cooling time should be and tell you whether the limit is the mould temperature, the contact, or the demould temperature.

Talk to a thermoforming engineer

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
it_ITIT

Chiedete un preventivo rapido

Inviare disegni e requisiti dettagliati via

Emial: [email protected]

Oppure compilate il modulo di contatto qui sotto: