{"id":9330,"date":"2024-01-14T01:00:00","date_gmt":"2024-01-14T01:00:00","guid":{"rendered":"https:\/\/uplastech.com\/profile-storage-blocking-stack-heat\/"},"modified":"2026-11-08T08:12:01","modified_gmt":"2026-11-08T08:12:01","slug":"profile-storage-blocking-stack-heat","status":"publish","type":"post","link":"https:\/\/uplastech.com\/id\/profile-storage-blocking-stack-heat\/","title":{"rendered":"Stacked PVC profiles blocking at 55 \u00b0C: stack pressure, not a bad compound"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n\/* ==UPL-CONVERSION-MODULES-START== 2024 problem-solving \/ lead-gen blocks *\/\n.upl-blog .mod-h{font-size:12.5px;letter-spacing:.12em;text-transform:uppercase;font-weight:700;color:#0d5563;margin:0 0 12px}\n.upl-blog .problem{background:#fff8f3;border:1px solid #f3ddc9;border-left:4px solid #e07a1f;border-radius:10px;padding:22px 26px;margin:0 0 32px;font-size:16px}\n.upl-blog .problem p{margin:0 0 10px}\n.upl-blog .problem p:last-child{margin-bottom:0}\n.upl-blog .problem .mod-h{color:#a85c10}\n.upl-blog .problem .problem-promise{font-weight:700;color:#0b2b33}\n.upl-blog .steps{background:#f7fafb;border:1px solid #e1ebee;border-radius:10px;padding:22px 26px;margin:0 0 28px}\n.upl-blog .steps ol{list-style:none;counter-reset:uplst;margin:0;padding:0}\n.upl-blog .steps li{counter-increment:uplst;position:relative;padding:0 0 16px 42px;margin:0;font-size:15.5px}\n.upl-blog .steps li:last-child{padding-bottom:0}\n.upl-blog .steps li::before{content:counter(uplst);position:absolute;left:0;top:2px;width:26px;height:26px;border-radius:50%;background:#0d5563;color:#fff;font-size:13px;font-weight:700;line-height:26px;text-align:center}\n.upl-blog table.spec th{background:#14707f}\n.upl-blog .conv{background:#eef6f7;border:1px solid #cfe4e8;border-radius:10px;padding:24px 26px;margin:32px 0}\n.upl-blog .conv p{margin:0 0 12px;font-size:15.5px}\n.upl-blog .conv .conv-lbl{font-weight:700;color:#0b2b33;margin:16px 0 8px}\n.upl-blog ul.conv-need{list-style:none;padding:0;margin:0 0 20px;display:grid;grid-template-columns:1fr 1fr;gap:6px 18px}\n.upl-blog ul.conv-need li{position:relative;padding-left:20px;margin:0;font-size:14.5px}\n.upl-blog ul.conv-need li::before{content:\"\";position:absolute;left:0;top:9px;width:9px;height:9px;border:2px solid #14707f;border-radius:2px}\n.upl-blog .conv-btn{display:inline-block;background:#0d5563;color:#fff;text-decoration:none;font-weight:700;padding:11px 22px;border-radius:7px;font-size:15px}\n.upl-blog .checklist{background:#fbfcfd;border:1px solid #e3e9ec;border-radius:10px;padding:24px 26px;margin:36px 0}\n.upl-blog .checklist ul{list-style:none;padding:0;margin:0 0 12px}\n.upl-blog .checklist li{position:relative;padding-left:28px;margin:0 0 10px;font-size:15.5px}\n.upl-blog .checklist li::before{content:\"\";position:absolute;left:0;top:7px;width:14px;height:14px;border:2px solid #0d5563;border-radius:3px}\n.upl-blog .cl-note{font-size:13.5px;color:#6b7280;margin:0}\n.upl-blog .cta .cta-lbl{color:#c9dee3;font-weight:700;margin:0 0 8px;font-size:14.5px}\n.upl-blog ul.cta-need{list-style:none;padding:0;margin:0 0 22px;display:grid;grid-template-columns:1fr 1fr;gap:4px 18px}\n.upl-blog ul.cta-need li{color:#e4f0f2;font-size:14.5px;padding-left:18px;position:relative;margin:0}\n.upl-blog ul.cta-need li::before{content:\"\\2713\";position:absolute;left:0;color:#e07a1f;font-weight:700}\n\/* ==UPL-CONVERSION-MODULES-END== *\/\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}.upl-blog ul.conv-need,.upl-blog ul.cta-need{grid-template-columns:1fr}.upl-blog .problem,.upl-blog .steps,.upl-blog .conv,.upl-blog .checklist{padding:18px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/2024-profile-storage-blocking-stack-heat-hero.jpg\" alt=\"Real extruded plastic profiles and pipe on a production site\" width=\"1536\" height=\"909\"><figcaption>Real plastic profile extrusion production context. Photo: Pexels.<\/figcaption><\/figure>\n<div class=\"problem\">\n<p class=\"mod-h\">The problem<\/p>\n<p><b>Symptom.<\/b> A fabricator opens a pallet of white PVC trim after three weeks in a warehouse that logged 55 \u00b0C and finds the bottom 18 layers stuck together, peeling at 3.2 N\/25 mm.<\/p>\n<p><b>What it costs.<\/b> Separating blocked lengths tears the decorative face and scraps 18 layers of a 50-layer stack, while the supplier points to a storage clause that never named a temperature limit.<\/p>\n<p class=\"problem-promise\">This guide ties blocking to stack pressure and temperature, and gives the four numbers to write into the storage and packing clause.<\/p>\n<\/div>\n<div class=\"toc\"><\/div>\n<h2 id=\"read-the-temperature-logger-before-you-blame-the-compound\">Read the temperature logger before you blame the compound<\/h2>\n<p>Blocking is pressure-assisted surface tack. A 6 m length of 6.0 kg in a 50-layer stack loads the bottom interface with P = 49 x 6.0 kg x 9.81 m\/s2 \/ 0.30 m2 = 9.6 kPa, enough to weld two warm faces.<\/p>\n<table>\n<thead>\n<tr>\n<th>Storage temperature (\u00b0C)<\/th>\n<th>Blocking peel force (N\/25 mm)<\/th>\n<th>Layers separating cleanly (%)<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>40 (controlled store)<\/td>\n<td>0.2<\/td>\n<td>100<\/td>\n<\/tr>\n<tr>\n<td>45 (clause limit)<\/td>\n<td>0.4<\/td>\n<td>99<\/td>\n<\/tr>\n<tr>\n<td>50<\/td>\n<td>1.5<\/td>\n<td>72<\/td>\n<\/tr>\n<tr>\n<td>55 (hot warehouse)<\/td>\n<td>3.2<\/td>\n<td>28<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 - Storage temperature against blocking peel force and stack recovery<\/p>\n<div class=\"callout\">Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.<\/div>\n<p><!-- upl-conv-v1 quickcta --><\/p>\n<div class=\"quickcta\">\n<p class=\"mod-h\">Need a fixed price for this profile?<\/p>\n<p>Send the cross-section drawing, material, cut length and annual volume. We will review die, calibration and tolerance, then return a written tooling and production quotation.<\/p>\n<p class=\"quickcta-act\"><a class=\"quickcta-btn\" href=\"https:\/\/uplastech.com\/plastic-extrusion-solutions\/\">Get a profile quotation<\/a><a class=\"quickcta-alt\" href=\"mailto:john@uplastech.com\">Email john@uplastech.com<\/a><a class=\"quickcta-alt\" href=\"https:\/\/wa.me\/8617717529949\">WhatsApp<\/a><\/p>\n<\/div>\n<h2 id=\"trace-the-tack-from-stack-pressure-to-the-face\">Trace the tack from stack pressure to the face<\/h2>\n<p>Treat the split below as illustrative engineering guidance, not a measured survey. Typically a blocked stack traces to a hot store, an over-high stack, no slip additive and missing interleaves, so read the temperature logger before questioning the compound.<\/p>\n<div class=\"steps\">\n<p class=\"mod-h\">A five-step diagnostic sequence<\/p>\n<ol>\n<li><b>Read the logger first.<\/b><br \/>Pull the warehouse temperature record; a 55 \u00b0C peak against a 45 \u00b0C clause explains blocking before any compound is questioned.<\/li>\n<li><b>Count the layers.<\/b><br \/>Measure stack height; 50 layers of 6.0 kg put 9.6 kPa on the bottom interface, while 25 layers halve it to 4.7 kPa.<\/li>\n<li><b>Peel a blocked pair.<\/b><br \/>Pull two stuck lengths at 180 degrees with a spring gauge; 3.2 N\/25 mm against a 1.0 N\/25 mm limit confirms pressure-assisted tack.<\/li>\n<li><b>Check slip additive and interleaf.<\/b><br \/>Confirm 0.15% erucamide and a kraft sheet per layer; 0% slip peaks at 3.2 N\/25 mm at 55 \u00b0C.<\/li>\n<li><b>Write the storage clause.<\/b><br \/>Specify 45 \u00b0C with a logger, 25 layers, 0.15% slip additive and interleaving so a blocked pallet is a temperature record, not a re-order.<\/li>\n<\/ol>\n<\/div>\n<p>The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.<\/p>\n<figure>\n<img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/profile-storage-blocking-stack-heat-chart.jpg\" alt=\"Stacked PVC profiles blocking at 55 \u00b0C: stack pressure, not a bad compound: calculated response trend and an illustrative root-cause split\" width=\"1536\" height=\"909\"><figcaption>Figure 1 \u2014 Calculated response trend and an illustrative root-cause split. Values are engineering guidance for diagnosis, not a measured survey; confirm them on your own line before changing a drawing or a specification.<\/figcaption><\/figure>\n<h2 id=\"set-the-storage-and-packing-parameters\">Set the storage and packing parameters<\/h2>\n<p>Four settings keep layers free: storage below 45 \u00b0C, a stack of 25 layers or less (4.7 kPa), 0.15% erucamide slip additive and a kraft interleaf every layer. Together they hold peel at 0.6 N\/25 mm even at 55 \u00b0C.<\/p>\n<table class=\"spec\">\n<thead>\n<tr>\n<th>Parameter<\/th>\n<th>Agreed value<\/th>\n<th>What goes wrong outside it<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Maximum storage temperature<\/td>\n<td>45 \u00b0C with logger<\/td>\n<td>At 55 \u00b0C peel force reaches 3.2 N\/25 mm<\/td>\n<\/tr>\n<tr>\n<td>Stack height \/ bottom pressure<\/td>\n<td>25 layers \/ 4.7 kPa<\/td>\n<td>50 layers reach 9.6 kPa and fuse the base<\/td>\n<\/tr>\n<tr>\n<td>Slip additive (erucamide)<\/td>\n<td>0.15% in the compound<\/td>\n<td>0% loading gives 3.2 N\/25 mm at 55 \u00b0C<\/td>\n<\/tr>\n<tr>\n<td>Interleaving<\/td>\n<td>Kraft sheet every layer<\/td>\n<td>Bare face-to-face contact blocks at the touch points<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 - Storage and packing settings that prevent blocking<\/p>\n<h2 id=\"prove-it-with-a-storage-dwell-trial\">Prove it with a storage-dwell trial<\/h2>\n<p>Run a storage-dwell trial with one lot: hold stacks at 40, 45, 50 and 55 \u00b0C for 21 days and peel at 180 degrees. Peel force reads 0.2, 0.4, 1.5 then 3.2 N\/25 mm, putting the 1.0 N\/25 mm limit near 47 \u00b0C.<\/p>\n<table>\n<thead>\n<tr>\n<th>Field symptom<\/th>\n<th>Most likely cause<\/th>\n<th>Check that confirms it<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Bottom layers fused, top layers free<\/td>\n<td>Stack pressure plus floor heat<\/td>\n<td>Logger reads 55 \u00b0C at the base of a 50-layer stack<\/td>\n<\/tr>\n<tr>\n<td>Whole stack tacky after a hot week<\/td>\n<td>Store above the 45 \u00b0C limit<\/td>\n<td>Warehouse logger peaked at 55 \u00b0C for 3 days<\/td>\n<\/tr>\n<tr>\n<td>Faces stick without a protective film<\/td>\n<td>No slip additive in the compound<\/td>\n<td>Peel reads 3.2 N\/25 mm at 0% erucamide<\/td>\n<\/tr>\n<tr>\n<td>Blocking only where layers touch<\/td>\n<td>No kraft interleaf between lengths<\/td>\n<td>Pallet shows bare face-to-face contact<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 - Matching blocked layers to the storage fault<\/p>\n<div class=\"myth\"><b>Myth:<\/b> \"A process adjustment will fix it.\" Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.<\/div>\n<h2 id=\"write-the-storage-clause-into-the-order\">Write the storage clause into the order<\/h2>\n<p>Write the storage clause into the order: a 45 \u00b0C ceiling with a data logger, a 25-layer stack limit, 0.15% slip additive and a kraft interleaf. Both parties reading one logger turn a blocked pallet into a temperature record, not an argument.<\/p>\n<div class=\"conv\">\n<p class=\"mod-h\">Need the section checked before tooling?<\/p>\n<p>Send us the section and the installation conditions. We will review wall balance, tolerance and fixing detail, then return a marked-up drawing with a tooling quotation.<\/p>\n<p class=\"conv-lbl\">What to send us<\/p>\n<ul class=\"conv-need\">\n<li>Cross-section drawing with wall thicknesses<\/li>\n<li>Material and colour<\/li>\n<li>Installation temperature range<\/li>\n<li>Fixing method and run length<\/li>\n<\/ul>\n<p><a class=\"conv-btn\" href=\"\/plastic-extrusion-solutions\/\">Send the section drawing<\/a>\n<\/div>\n<h2 id=\"what-a-cool-store-saves-over-a-summer-season\">What a cool store saves over a summer season<\/h2>\n<p>A cool store protects the face. A 0.15% slip dose costs little against 18 scrapped layers; holding 45 \u00b0C keeps peel near 0.4 N\/25 mm and 99% of layers free, while one hot week can fuse a whole stack before it is opened.<\/p>\n<div class=\"callout\">Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.<\/div>\n<div class=\"checklist\">\n<p class=\"mod-h\">Before you release this extruded profile<\/p>\n<ul>\n<li>A 45 \u00b0C storage ceiling with a data logger is written into the order<\/li>\n<li>A 25-layer stack limit and 4.7 kPa bottom pressure are stated<\/li>\n<li>0.15% erucamide slip additive is required in the compound<\/li>\n<li>A kraft interleaf between every layer appears in the packing spec<\/li>\n<li>A 1.0 N\/25 mm maximum blocking peel force is the acceptance test<\/li>\n<\/ul>\n<p class=\"cl-note\">Write the measurement temperature and the tolerance into the drawing; most disputes are really about how the part was measured.<\/p>\n<\/div>\n<div class=\"faq\">\n<h3>Why do my stacked PVC profiles stick together?<\/h3>\n<p>Heat and pressure. A warehouse at 55 \u00b0C softens the face while a 50-layer stack loads the bottom with about 9.6 kPa, so peel force reaches 3.2 N\/25 mm instead of 0.4.<\/p>\n<h3>Is blocking a compound fault?<\/h3>\n<p>Partly. A 0.15% erucamide slip additive cuts peel from 3.2 to 0.6 N\/25 mm at 55 \u00b0C, but even a good compound blocks above 45 \u00b0C under a tall stack.<\/p>\n<h3>How much does stack height matter?<\/h3>\n<p>Pressure scales with layers. P = 49 x 6.0 kg x 9.81 m\/s2 \/ 0.30 m2 = 9.6 kPa at 50 layers, falling to 4.7 kPa when the stack is halved to 25.<\/p>\n<h3>What storage temperature should the clause allow?<\/h3>\n<p>45 \u00b0C maximum with a logger. At 45 \u00b0C peel holds near 0.4 N\/25 mm and 99% of layers separate cleanly; at 50 \u00b0C it already reaches 1.5 N\/25 mm.<\/p>\n<h3>Do I need an interleaf?<\/h3>\n<p>Yes for a hot climate. A kraft sheet every layer removes bare face-to-face contact, which is where a 3.2 N\/25 mm bond starts even with slip additive.<\/p>\n<h3>What should the acceptance test say?<\/h3>\n<p>A 45 \u00b0C ceiling with a logger, 25 layers, 0.15% slip additive, interleaving, and blocking peel force below 1.0 N\/25 mm measured at 180 degrees after 21 days.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Get a profile that holds its dimension<\/p>\n<p>Send us the profile section, the length and the service conditions. We will review die, calibration and tolerance, then quote tooling and production with a defined measurement method.<\/p>\n<p class=\"cta-lbl\">To get an accurate quote, send:<\/p>\n<ul class=\"cta-need\">\n<li>Profile cross-section drawing<\/li>\n<li>Material and colour<\/li>\n<li>Cut length and annual volume<\/li>\n<li>Service temperature and exposure<\/li>\n<\/ul>\n<p><a class=\"btn\" href=\"\/plastic-extrusion-solutions\/\">Request a profile quotation<\/a><br \/>\n<!-- upl-conv-v1 contact --><\/p>\n<div class=\"contactbar\">\n<p class=\"contactbar-h\">Prefer to talk it through first?<\/p>\n<p>Email <a href=\"mailto:john@uplastech.com\">john@uplastech.com<\/a> or message us on <a href=\"https:\/\/wa.me\/8617717529949\">WhatsApp +86 177 1752 9949<\/a>. Send a drawing, a sample or a specification and an engineer will reply.<\/p>\n<\/div>\n<p><!-- upl-conv-v1 trust --><\/p>\n<div class=\"trust\">\n<p class=\"trust-h\">Why buyers work with Uplastech<\/p>\n<p>ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.<\/p>\n<\/div>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/extrusion-dimensional-drift\/\">Extrusion dimensional drift<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/extrusion-profile-tolerance\/\">Extrusion profile tolerance<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/profile-calibration-cooling\/\">Profile calibration and cooling<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pvc-profile-weathering-colour\/\">PVC profile weathering and colour<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/pvc-window-profile-design\/\">PVC window profile design<\/a><\/li>\n<\/ul>\n<p><!-- upl-conv-v1 service --><\/p>\n<p class=\"rel-svc\">Ready to specify? See our <a href=\"https:\/\/uplastech.com\/plastic-extrusion-solutions\/\">plastic profile extrusion services<\/a> or <a href=\"mailto:john@uplastech.com\">request a written quotation<\/a>.<\/p>\n<\/div>\n<\/div>\n<p><script type=\"application\/ld+json\">{\"@context\": \"https:\/\/schema.org\", \"@type\": \"FAQPage\", \"mainEntity\": [{\"@type\": \"Question\", \"name\": \"Why do my stacked PVC profiles stick together?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"Heat and pressure. A warehouse at 55 \u00b0C softens the face while a 50-layer stack loads the bottom with about 9.6 kPa, so peel force reaches 3.2 N\/25 mm instead of 0.4.\"}}, {\"@type\": \"Question\", \"name\": \"Is blocking a compound fault?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"Partly. A 0.15% erucamide slip additive cuts peel from 3.2 to 0.6 N\/25 mm at 55 \u00b0C, but even a good compound blocks above 45 \u00b0C under a tall stack.\"}}, {\"@type\": \"Question\", \"name\": \"How much does stack height matter?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"Pressure scales with layers. P = 49 x 6.0 kg x 9.81 m\/s2 \/ 0.30 m2 = 9.6 kPa at 50 layers, falling to 4.7 kPa when the stack is halved to 25.\"}}, {\"@type\": \"Question\", \"name\": \"What storage temperature should the clause allow?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"45 \u00b0C maximum with a logger. At 45 \u00b0C peel holds near 0.4 N\/25 mm and 99% of layers separate cleanly; at 50 \u00b0C it already reaches 1.5 N\/25 mm.\"}}, {\"@type\": \"Question\", \"name\": \"Do I need an interleaf?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"Yes for a hot climate. A kraft sheet every layer removes bare face-to-face contact, which is where a 3.2 N\/25 mm bond starts even with slip additive.\"}}, {\"@type\": \"Question\", \"name\": \"What should the acceptance test say?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"A 45 \u00b0C ceiling with a logger, 25 layers, 0.15% slip additive, interleaving, and blocking peel force below 1.0 N\/25 mm measured at 180 degrees after 21 days.\"}}]}<\/script><\/p>\n","protected":false},"excerpt":{"rendered":"<p>This guide ties blocking to stack pressure and temperature, and gives the four numbers to write into the storage and packing clause.<\/p>","protected":false},"author":1,"featured_media":9328,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[17],"tags":[],"class_list":["post-9330","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-plastic-extrusion-process"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/posts\/9330","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/comments?post=9330"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/posts\/9330\/revisions"}],"predecessor-version":[{"id":9916,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/posts\/9330\/revisions\/9916"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/media\/9328"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/media?parent=9330"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/categories?post=9330"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/tags?post=9330"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}