{"id":8294,"date":"2026-04-04T09:00:00","date_gmt":"2026-04-04T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/silicone-tearing-defect\/"},"modified":"2026-04-04T09:00:00","modified_gmt":"2026-04-04T08:00:00","slug":"silicone-tearing-defect","status":"publish","type":"post","link":"https:\/\/uplastech.com\/id\/silicone-tearing-defect\/","title":{"rendered":"Tearing in Silicone Parts: Demoulding Force and the Undercut Nobody Drew"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/silicone-tearing-defect.jpg\" alt=\"Moulded white silicone parts on a bench, two clean and two with torn ragged edges, a gloved hand comparing a torn part with a good one, a demoulding hook beside them\" width=\"1536\" height=\"909\"><figcaption>Two good parts and two torn ones from the same tool. The tear always starts at the same place, which is the clue.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"force\">Tearing is a force problem<\/h2>\n<p>Silicone tears when the force needed to remove it from the tool exceeds its tear strength at the point where the force is concentrated. Both halves of that sentence matter: the force comes from the tool, and the concentration comes from the geometry.<\/p>\n<p>The force has three sources. The interference fit over an undercut, which is the largest and the one that is usually not on the drawing. The friction on the walls, which depends on the shrinkage and the surface finish. And the adhesion to the tool, which is small unless the tool is dirty or the release agent is wrong.<\/p>\n<p>The concentration has two sources. A thin section, which has less material to carry the load. And a sharp corner, which multiplies the stress. A part with a 0.5 mm section and a 0.2 mm radius will tear at a force that a 2 mm section would shrug off.<\/p>\n<p>So the diagnosis starts with where the tear is. A tear at the edge of a thin section is a section problem. A tear at the base of a feature is an undercut problem. A tear that is random across the part is a temperature or a release problem.<\/p>\n<h2 id=\"temperature\">Demould temperature is the first lever<\/h2>\n<p>A silicone part is weakest when it is hot. The tear strength of a typical 50 Shore A compound at 160 C is about 60 percent of its room temperature value, and at 190 C it is about 35 percent. So a part demoulded hot is a part that tears at a force it would survive cold.<\/p>\n<p>The measured tear rate follows that. At 150 C it is 0.4 percent. At 160 it is 0.6, at 170 it is 1.5, at 180 it is 4.2, and at 190 it is 9.8. Between 160 and 190 the rate goes up by a factor of sixteen for 30 C.<\/p>\n<p>The obvious fix is to demould cooler, and the cost is cycle time. A part that is demoulded at 160 C instead of 190 C needs 20 to 40 seconds more cooling, which on a 90 second cycle is a 25 to 45 percent throughput loss. That is why the compromise is usually 170 to 175 C, where the tear rate is 1.5 to 2.5 percent and the cycle is still competitive.<\/p>\n<p>The other temperature to check is uniformity. A part that is cool at the edge and hot in the middle tears at the edge, because the edge is being pulled while the middle is still soft and moving. A tool with uneven cooling produces a tear pattern that follows the temperature map.<\/p>\n<figure>\n<img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/silicone-tearing-defect-chart.jpg\" alt=\"Tear rate rising from 0.4 percent at a 150 C demould to 9.8 percent at 190 C, and demould force rising from 12 newtons with no undercut to 198 newtons at 1 mm of undercut\" width=\"1536\" height=\"909\"><figcaption>Left: tear rate against demould temperature, 0.4 percent at 150 C and 9.8 at 190. Right: demould force against undercut on the core, 12 N with no undercut and 198 N at 1 mm, with the strip-safe zone below about 60 N.<\/figcaption><\/figure>\n<h2 id=\"undercut\">The undercut nobody drew<\/h2>\n<p>An undercut is any feature that the part has to stretch over to come off the core. A designed one is a snap fit or a sealing bead. An undesigned one is a tool feature that was added for another reason and happens to interfere.<\/p>\n<p>The common undesigned undercuts are a draft that is reversed on one wall, a polishing mark that has been blended into an edge, a text engraving with vertical walls, and an ejector pin that stands 0.05 mm proud. None of them look like an undercut on the drawing and all of them cost force.<\/p>\n<p>The force is large. With no undercut the demould force is about 12 newtons. At 0.2 mm it is 26, at 0.4 mm 48, at 0.6 mm 82, at 0.8 mm 131, and at 1.0 mm 198. The relationship is not linear: doubling from 0.4 to 0.8 mm nearly triples the force, because the silicone has to stretch further and its modulus rises as it does.<\/p>\n<p>A 60 newton limit is a reasonable working ceiling for hand demoulding, and it corresponds to about 0.45 mm of undercut. Beyond that the part needs a stripping tool or a redesign, and a part that is stripped by hand at 130 newtons is a part that is torn by the operator on a bad day.<\/p>\n<p>Finding the undercut is a matter of measurement, not inspection. A dial indicator run around the core at the point where the tear starts will show a step of 0.05 to 0.2 mm that the eye does not. A blue-marking compound rubbed on the core and then checked on the part shows exactly where it is gripping.<\/p>\n<table>\n<thead>\n<tr>\n<th>Undercut<\/th>\n<th>Demould force<\/th>\n<th>How to remove the part<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>None<\/td>\n<td>12 N<\/td>\n<td>Hand, no effort<\/td>\n<\/tr>\n<tr>\n<td>0.2 mm<\/td>\n<td>26 N<\/td>\n<td>Hand<\/td>\n<\/tr>\n<tr>\n<td>0.4 mm<\/td>\n<td>48 N<\/td>\n<td>Hand, firm pull<\/td>\n<\/tr>\n<tr>\n<td>0.6 mm<\/td>\n<td>82 N<\/td>\n<td>Stripping tool<\/td>\n<\/tr>\n<tr>\n<td>0.8 mm<\/td>\n<td>131 N<\/td>\n<td>Stripping tool, risk of tear<\/td>\n<\/tr>\n<tr>\n<td>1.0 mm<\/td>\n<td>198 N<\/td>\n<td>Redesign or split tool<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 What an undercut costs in demould force<\/p>\n<h2 id=\"geometry\">Geometry that concentrates the force<\/h2>\n<p>A tear needs a place to start. On a smooth, generous part the force is spread over an area and the stress is low. On a part with a thin section and a sharp corner the same force is concentrated into a few square millimetres and the stress is above the tear strength.<\/p>\n<p>The rule is that every internal corner should have a radius of at least half the section thickness, and every external corner at least the section thickness. A 1 mm section with a 0.2 mm internal radius has a stress concentration of about 3.5; the same section with a 0.5 mm radius has about 1.8.<\/p>\n<p>Thin sections are the other half. A silicone part with a 0.3 mm wall is a part that will tear at a demould force that a 1 mm wall would ignore, because the force is carried by a tenth of the material. A thin wall is often a design requirement, and the answer is a stripping tool rather than a hand pull.<\/p>\n<p>The parting line is a third. A parting line that is not flush leaves a step, and a step is an undercut. A tool with a 0.05 mm mismatch at the parting line is a tool with a 0.05 mm undercut all the way round the part, and that is enough to double the demould force on a large part.<\/p>\n<h2 id=\"release\">Release, and the things that are not the tool<\/h2>\n<p>A tear that is random across the part, rather than at a feature, is usually a release problem. The part is sticking to the cavity as well as the core, so the demould force is pulling against two surfaces and the part tears where it is weakest.<\/p>\n<p>The causes are a tool that needs cleaning, a release agent that has been applied unevenly, an internal release agent that has been washed out of the compound, or a compound that is under-cured. An under-cured part is soft and tacky and it tears at a fraction of the force a fully cured part would take.<\/p>\n<p>Cure is worth checking before the tool. A part that is 10 percent under-cured has a tear strength about 25 percent lower and a surface that is slightly tacky. The cure can be checked with a hardness reading, a compression set test or a simple tear by hand on a test piece, and it takes minutes.<\/p>\n<p>The release agent itself is a variable that is easy to get wrong. A silicone release agent on a silicone part is a contamination risk; a solvent-based one that has not flashed off is a mould that is wet. The right amount is a thin film that is almost invisible, applied to a clean tool at the start of a run and not every cycle.<\/p>\n<h2 id=\"fix\">Fixing it in the right order<\/h2>\n<p>Start with the demould temperature. If the part is coming out at 185 C and the tear rate is 5 percent, dropping to 170 C will take it to about 1.5 percent and the cost is 20 seconds of cycle. That is the cheapest fix and it is usually enough.<\/p>\n<p>Then check the cure. A part that is under-cured tears at a lower force and it feels tacky. A hardness reading against the specification takes a minute and it eliminates a whole class of causes.<\/p>\n<p>Then measure the undercut. A dial indicator around the core at the tear point will find a step that the eye cannot, and a step of 0.1 mm is 12 newtons of force on its own.<\/p>\n<p>Then look at the geometry. A thin section or a sharp corner at the tear point needs a radius or a thickness change, and that is a tool modification rather than a process change.<\/p>\n<table>\n<thead>\n<tr>\n<th>Where it tears<\/th>\n<th>What it means<\/th>\n<th>First fix<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Base of a feature<\/td>\n<td>Undercut<\/td>\n<td>Measure the step, add draft<\/td>\n<\/tr>\n<tr>\n<td>Edge of a thin wall<\/td>\n<td>Section too thin<\/td>\n<td>Thicken, or strip with a tool<\/td>\n<\/tr>\n<tr>\n<td>Sharp internal corner<\/td>\n<td>Stress concentration<\/td>\n<td>Add a radius<\/td>\n<\/tr>\n<tr>\n<td>Along the parting line<\/td>\n<td>Parting line step<\/td>\n<td>Flush the parting line<\/td>\n<\/tr>\n<tr>\n<td>Random across the part<\/td>\n<td>Release or cure<\/td>\n<td>Check hardness and tool condition<\/td>\n<\/tr>\n<tr>\n<td>Always on the same cavity<\/td>\n<td>That cavity's tool<\/td>\n<td>Inspect that core<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 Reading the tear by where it starts<\/p>\n<div class=\"myth\">Myth: silicone tears because it is a soft material, and a harder compound will fix it. A harder compound has a higher tear strength and a higher modulus, so the demould force goes up as well. The tear rate often does not change, and the part is now harder than the application wanted. Tearing is a force and geometry problem, not a hardness problem.<\/div>\n<div class=\"faq\">\n<h3>Why do silicone parts tear on demould?<\/h3>\n<p>Because the force needed to remove the part exceeds the tear strength where the force is concentrated. The force comes from an undercut or friction; the concentration comes from a thin section or a sharp corner.<\/p>\n<h3>How much does demould temperature matter?<\/h3>\n<p>A lot. The tear rate is 0.6 percent at 160 C and 9.8 percent at 190, because silicone loses about two thirds of its tear strength between those temperatures.<\/p>\n<h3>How much undercut can a part take?<\/h3>\n<p>About 0.45 mm for hand demoulding, which is 60 newtons. At 1 mm the force is 198 newtons and the part needs a stripping tool or a redesign.<\/p>\n<h3>How do I find an undercut that is not on the drawing?<\/h3>\n<p>Run a dial indicator around the core at the point where the tear starts. A step of 0.05 to 0.2 mm will show, and a blue-marking compound rubbed on the core shows where it grips.<\/p>\n<h3>Will a harder compound stop the tearing?<\/h3>\n<p>Not usually. A harder compound has a higher tear strength and a higher modulus, so the demould force rises too. The tear rate often stays the same and the part is now harder than the application wanted.<\/p>\n<h3>What if the tears are random across the part?<\/h3>\n<p>That is a release or a cure problem. The part is sticking to both halves, or it is under-cured and soft. Check the hardness and the cure before touching the tool.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">A part that tears at the same place every time?<\/p>\n<p>Send a photo of the tear, the demould temperature and the tool drawing. We will tell you whether it is an undercut, a thin section or a cure problem.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/id\/silicone-rubber\/\">Ask about silicone moulding<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/id\/silicone-mold-design\/\">Silicone Mold Design: Shrinkage, Parting and Ejection<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/id\/silicone-mold-release\/\">Silicone Mold Release: Agents, Build-Up and Contamination<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/id\/silicone-compression-molding\/\">Silicone Compression Molding: Charge, Vent and Cure<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/id\/silicone-hardness-shore-a\/\">Silicone Hardness Shore A: What the Number Actually Means<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/id\/silicone-rubber\/\">Silicone Rubber Products: Moulded, Extruded and Calendered<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>A part demoulded at 190 C tears 9.8 percent of the time and one at 160 C tears 0.6. And every millimetre of undercut on the core costs 198 newtons of demould force, which is where the tear actually starts.<\/p>","protected":false},"author":1,"featured_media":8292,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[39],"tags":[],"class_list":["post-8294","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-silicone-rubber-products"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/posts\/8294","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/comments?post=8294"}],"version-history":[{"count":0,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/posts\/8294\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/media\/8292"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/media?parent=8294"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/categories?post=8294"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/id\/wp-json\/wp\/v2\/tags?post=8294"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}