{"id":7679,"date":"2025-08-16T09:00:00","date_gmt":"2025-08-16T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/packing-pressure-hold-time\/"},"modified":"2025-08-16T09:00:00","modified_gmt":"2025-08-16T08:00:00","slug":"packing-pressure-hold-time","status":"publish","type":"post","link":"https:\/\/uplastech.com\/fr\/packing-pressure-hold-time\/","title":{"rendered":"Packing Pressure and Hold Time: How to Set Them From the Part"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u81ea\u52a8\u5c55\u5f00\u7684\u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/packing-pressure-hold-time.jpg\" alt=\"Chart of cavity pressure against time showing gate freeze point and the effect of different hold times on part weight\" width=\"1536\" height=\"909\"><figcaption>Cavity pressure rises during filling, drops at the switchover, then holds flat while the gate is open. The moment it starts to fall is gate freeze \u2014 and it is the only correct hold time.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"what\">What packing actually does<\/h2>\n<p>When the screw stops, the cavity is full but the part is not finished. The polymer is cooling and shrinking, and that shrinkage has to be made up with more material \u2014 otherwise the part pulls away from the cavity walls, sinks, and ends up underweight and undersized.<\/p>\n<p>Packing pressure does that make-up. It pushes additional melt through the still-open gate to compensate for shrinkage. Hold time is how long that pressure is maintained. Both are set by the part, not by preference, and both have an exact correct answer that can be measured.<\/p>\n<div class=\"callout\">\n<p><strong>The single most useful measurement in injection moulding:<\/strong> cavity pressure at the gate. It rises through filling, drops when the machine switches from velocity to pressure control, holds flat while the gate is open, and then falls when the gate freezes. That falling edge is gate freeze, and it is where hold time should end.<\/p>\n<\/div>\n<h2 id=\"three-phases\">The three phases of packing<\/h2>\n<table>\n<thead>\n<tr>\n<th>Phase<\/th>\n<th>What happens<\/th>\n<th>Time scale<\/th>\n<th>Controlled by<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Filling<\/td>\n<td>Cavity fills, pressure rises<\/td>\n<td>0.5 \u2013 3 s<\/td>\n<td>Injection velocity profile<\/td>\n<\/tr>\n<tr>\n<td>Compression \/ switchover<\/td>\n<td>Velocity control hands over to pressure control; peak cavity pressure<\/td>\n<td>0.1 \u2013 0.5 s<\/td>\n<td>Switchover point and pack pressure setting<\/td>\n<\/tr>\n<tr>\n<td>Packing \/ holding<\/td>\n<td>Additional melt enters through the gate to offset shrinkage<\/td>\n<td>2 \u2013 20 s<\/td>\n<td>Hold pressure and hold time<\/td>\n<\/tr>\n<tr>\n<td>Gate freeze<\/td>\n<td>Gate solidifies; no more material can enter<\/td>\n<td>\u2014<\/td>\n<td>Gate geometry and cooling<\/td>\n<\/tr>\n<tr>\n<td>Refroidissement<\/td>\n<td>Part cools with no further mass change<\/td>\n<td>Until ejection<\/td>\n<td>Temps de refroidissement<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 The phases of a cycle after filling. Everything after gate freeze is cooling, and extending hold beyond gate freeze does nothing except waste time.<\/p>\n<p>Gate freeze is the pivot. Before it, hold pressure controls part weight and dimensions. After it, hold pressure has no effect at all, because there is no path for material to enter. Running hold time past gate freeze is the most common wasted second in injection moulding.<\/p>\n<h2 id=\"finding\">Finding gate freeze<\/h2>\n<p>There are two ways: with a cavity pressure sensor, and without one. The sensor method is faster and more accurate; the weight method works on any machine.<\/p>\n<p><strong>With a sensor.<\/strong> Plot cavity pressure against time. The pressure holds flat during packing and then drops when the gate freezes and the part starts to shrink away from the sensor. The time at which the drop begins is gate freeze.<\/p>\n<p><strong>Without a sensor.<\/strong> Run a series of parts at increasing hold times, weighing each one. Part weight rises with hold time and then plateaus. The point where the curve flattens is gate freeze. It takes six to eight parts and about twenty minutes, and it needs no instrumentation.<\/p>\n<table>\n<thead>\n<tr>\n<th>Hold time (s)<\/th>\n<th>Part weight (g)<\/th>\n<th>Interpretation<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1.0<\/td>\n<td>24.82<\/td>\n<td>Short \u2014 sink likely<\/td>\n<\/tr>\n<tr>\n<td>2.0<\/td>\n<td>25.31<\/td>\n<td>Still filling out<\/td>\n<\/tr>\n<tr>\n<td>3.0<\/td>\n<td>25.64<\/td>\n<td>Approaching plateau<\/td>\n<\/tr>\n<tr>\n<td>4.0<\/td>\n<td>25.78<\/td>\n<td>Near plateau<\/td>\n<\/tr>\n<tr>\n<td>5.0<\/td>\n<td>25.81<\/td>\n<td>Plateau<\/td>\n<\/tr>\n<tr>\n<td>6.0<\/td>\n<td>25.82<\/td>\n<td>Plateau \u2014 gate frozen at ~5 s<\/td>\n<\/tr>\n<tr>\n<td>8.0<\/td>\n<td>25.82<\/td>\n<td>No change; 3 s wasted<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 The weight-plateau method. Gate freeze is where the weight stops changing, which here is about 5 seconds. Hold time should be set at 5 seconds, not 8.<\/p>\n<p>The plateau method has one subtlety: it must be run at the intended pack pressure. At a low pack pressure the gate may freeze earlier because less hot melt is flowing through it; at a high pack pressure the gate stays open longer. Set pack pressure first, then find gate freeze.<\/p>\n<h2 id=\"setting-pressure\">Setting pack pressure<\/h2>\n<p>Pack pressure is expressed as a percentage of injection pressure on most machines, which makes it machine-specific and not portable between presses. The useful number is cavity pressure, and the useful target is a part that is dimensionally correct and visually acceptable.<\/p>\n<table>\n<thead>\n<tr>\n<th>Pack pressure<\/th>\n<th>Effect on part<\/th>\n<th>Symptoms<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Too low<\/td>\n<td>Insufficient material added<\/td>\n<td>Sink, voids, short shots, undersize, warpage<\/td>\n<\/tr>\n<tr>\n<td>Correct<\/td>\n<td>Weight at plateau, dimensions on nominal<\/td>\n<td>None<\/td>\n<\/tr>\n<tr>\n<td>Too high<\/td>\n<td>Over-packed; stress and flash<\/td>\n<td>Flash, ejection damage, high residual stress, warpage in the other direction<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 \u2014 Pack pressure effects. Both too low and too high cause warpage, which is why warpage alone does not tell you which way to go.<\/p>\n<p>The practical procedure is to start at a pressure that clearly produces a short shot or visible sink, then raise it in steps until the part is dimensionally correct and cosmetically acceptable, then check for flash. The correct setting is the lowest pressure that produces an acceptable part \u2014 not the highest that does not flash.<\/p>\n<p>Running at the lowest acceptable pressure matters because higher pack pressure means higher residual stress, which means more warpage and more stress cracking later. It also means more clamp force required and more wear on the tool.<\/p>\n<h2 id=\"profile\">Packing profiles<\/h2>\n<p>Single-stage packing is fine for simple parts. For parts with thick sections, ribs or a long flow path, a two-stage or three-stage profile gives better results.<\/p>\n<table>\n<thead>\n<tr>\n<th>Profile<\/th>\n<th>Forme<\/th>\n<th>Utilisation<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Single stage<\/td>\n<td>Constant pressure throughout hold<\/td>\n<td>Simple, uniform-wall parts<\/td>\n<\/tr>\n<tr>\n<td>Two stage (high then low)<\/td>\n<td>High pressure briefly, then reduced<\/td>\n<td>Parts with a thick section that must be packed before the gate freezes<\/td>\n<\/tr>\n<tr>\n<td>Three stage<\/td>\n<td>High, medium, low<\/td>\n<td>Thick parts with a long hold; reduces stress at the gate<\/td>\n<\/tr>\n<tr>\n<td>Ramp down<\/td>\n<td>Gradual decay<\/td>\n<td>Reduces gate stress marks; used on optical parts<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 4 \u2014 Packing profiles. The two-stage profile is the most common upgrade: it packs the thick section early while the gate is open, then reduces pressure to avoid over-packing the thin sections.<\/p>\n<p>The reason for reducing pressure later is that thin sections freeze first. Once they are solid, additional pressure cannot pack them, but it still acts on the gate area and on the still-molten core of thick sections. A high pressure held too long over-packs the gate region, which shows as a stress halo around the gate and sometimes as a small crack.<\/p>\n<h2 id=\"materials\">How the resin changes the numbers<\/h2>\n<table>\n<thead>\n<tr>\n<th>Resin<\/th>\n<th>Typical gate freeze<\/th>\n<th>Pack pressure (cavity)<\/th>\n<th>Notes<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>PP<\/td>\n<td>2 \u2013 4 s<\/td>\n<td>200 \u2013 400 bar<\/td>\n<td>High shrinkage; needs generous packing<\/td>\n<\/tr>\n<tr>\n<td>PE<\/td>\n<td>2 \u2013 5 s<\/td>\n<td>200 \u2013 400 bar<\/td>\n<td>Similar to PP<\/td>\n<\/tr>\n<tr>\n<td>PS<\/td>\n<td>2 \u2013 4 s<\/td>\n<td>200 \u2013 350 bar<\/td>\n<td>Low shrinkage; less critical<\/td>\n<\/tr>\n<tr>\n<td>ABS<\/td>\n<td>3 \u2013 6 s<\/td>\n<td>300 \u2013 500 bar<\/td>\n<td>Moderate; watch gate stress<\/td>\n<\/tr>\n<tr>\n<td>PC<\/td>\n<td>4 \u2013 8 s<\/td>\n<td>400 \u2013 700 bar<\/td>\n<td>High viscosity; needs high pressure<\/td>\n<\/tr>\n<tr>\n<td>PA66<\/td>\n<td>2 \u2013 4 s<\/td>\n<td>400 \u2013 800 bar<\/td>\n<td>Crystalline; freeze is fast once it starts<\/td>\n<\/tr>\n<tr>\n<td>POM<\/td>\n<td>3 \u2013 6 s<\/td>\n<td>400 \u2013 700 bar<\/td>\n<td>High crystallinity; significant shrinkage<\/td>\n<\/tr>\n<tr>\n<td>PBT<\/td>\n<td>2 \u2013 4 s<\/td>\n<td>400 \u2013 700 bar<\/td>\n<td>Fast freeze; short packing window<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 5 \u2014 Typical packing values by resin. The gate freeze times assume a 1.5\u20132 mm gate; a bigger gate stays open longer.<\/p>\n<p>Gate size is the strongest influence on freeze time, and it is fixed in the tool. A 1 mm gate on a 3 mm wall freezes in about a second, which leaves almost no packing window and produces sink no matter what the machine does. That is a tooling problem, and no process setting fixes it.<\/p>\n<h2 id=\"diagnose\">Diagnosing from the part<\/h2>\n<table>\n<thead>\n<tr>\n<th>D\u00e9faut<\/th>\n<th>What it suggests<\/th>\n<th>First adjustment<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Sink on a thick section<\/td>\n<td>Gate froze before the section was packed<\/td>\n<td>Longer hold, higher pressure, or a bigger gate<\/td>\n<\/tr>\n<tr>\n<td>Voids inside a thick section<\/td>\n<td>Same as sink, but the skin is stiff enough to hold<\/td>\n<td>Same; also check for moisture<\/td>\n<\/tr>\n<tr>\n<td>Flash at the parting line<\/td>\n<td>Pack pressure too high or clamp force too low<\/td>\n<td>Reduce pressure; check clamp tonnage<\/td>\n<\/tr>\n<tr>\n<td>L'arr\u00eat de travail<\/td>\n<td>Either over- or under-packed<\/td>\n<td>Check part weight against the plateau; then adjust<\/td>\n<\/tr>\n<tr>\n<td>Stress halo at the gate<\/td>\n<td>Over-packed, or pressure released too fast<\/td>\n<td>Profile the pressure down; slow the release<\/td>\n<\/tr>\n<tr>\n<td>Short shot at the end of flow<\/td>\n<td>Insufficient pressure, or gate froze early<\/td>\n<td>Raise pressure; check melt temperature<\/td>\n<\/tr>\n<tr>\n<td>Weight variation between shots<\/td>\n<td>Inconsistent switchover or check-ring leakage<\/td>\n<td>Check switchover repeatability and non-return valve<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 6 \u2014 Reading the part for packing problems. Weight variation is the most diagnostic: a stable process produces parts within 0.2% of each other.<\/p>\n<p>Part weight is the single best production indicator of packing stability. If the weight varies by more than about 0.3% between shots on a stable process, something is changing \u2014 switchover position, melt viscosity, or check-ring leakage. Weighing ten parts once an hour catches most packing problems before they become a customer complaint.<\/p>\n<div class=\"faq\">\n<h3>How do I find the right hold time?<\/h3>\n<p>Weigh parts at increasing hold times. The weight rises and then plateaus; the point where it flattens is gate freeze, and that is the correct hold time. With a cavity pressure sensor, watch for the pressure to start falling \u2014 same answer, faster.<\/p>\n<h3>What happens if hold time is too short?<\/h3>\n<p>The gate freezes before the part is fully packed. The result is sink on thick sections, internal voids, undersized dimensions and warpage. Short hold time is the most common cause of sink that appears \"for no reason\" on a part that used to run fine.<\/p>\n<h3>What happens if hold time is too long?<\/h3>\n<p>Nothing to the part, but you lose cycle time. Once the gate is frozen no more material can enter, so additional hold time has zero effect. On a 20-second cycle, running hold 3 seconds past gate freeze costs 15% of output for no benefit.<\/p>\n<h3>Should pack pressure be higher or lower than injection pressure?<\/h3>\n<p>Lower, typically 40\u201370% of injection pressure. Injection pressure is what it takes to fill the cavity at the required velocity; pack pressure only needs to compensate for shrinkage. Running pack at full injection pressure over-packs the part and causes flash.<\/p>\n<h3>Why does my part warp in one direction and sink in another?<\/h3>\n<p>Because different sections are packed differently. Thin sections freeze early and cannot be packed; thick sections stay open longer and receive more material. The differential shrinkage between them causes warpage. A packing profile or a wall-thickness change is the fix.<\/p>\n<h3>Does gate size affect packing?<\/h3>\n<p>Strongly. A larger gate stays molten longer, which gives a longer packing window and better sink control. A gate that freezes in under a second leaves almost no window. If a part cannot be packed, gate size is often the real problem.<\/p>\n<h3>How do I know if the check ring is leaking?<\/h3>\n<p>Part weight becomes inconsistent between shots, and the cushion (the amount of melt left in front of the screw at the end of hold) varies. A leaking check ring lets material flow back during packing, so the effective pack pressure is lower and variable.<\/p>\n<h3>Is cavity pressure control worth installing?<\/h3>\n<p>For high-volume precision parts, yes \u2014 it makes the process independent of material viscosity variation. For general purpose work, the weight-plateau method gives you the same information once, and hourly weighing maintains it.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Parts sinking, warping or varying in weight?<\/p>\n<p>Send us the part drawing, the resin, the gate size and your current pack settings. We will tell you whether the limit is the process or the tool, and what the correct hold time is for that gate.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/fr\/injection-molding\/\">Talk to a moulding engineer<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/fr\/injection-molding-cooling-time\/\">Cooling Time in Injection Molding: The Calculation That Sets Cycle Time<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/fr\/injection-molding-design-guidelines\/\">Injection Molding Design Guidelines: 12 Rules That Cut Part Cost<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/fr\/injection-molding-defects\/\">Injection Molding Defects: 12 Problems, Causes and Fixes<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/fr\/injection-mold-steel-selection\/\">Injection Mold Steel Selection: P20, H13, S136<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/fr\/injection-molding-tolerances\/\">Injection Molding Tolerances: What Is Actually Achievable<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Pack pressure is set by cavity pressure at gate freeze, not by a number on the controller. How to find gate freeze and what happens either side of it.<\/p>","protected":false},"author":1,"featured_media":7672,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_seopress_titles_title":"Packing Pressure and Hold Time: How to Set Them From the Par","_seopress_titles_desc":"Pack pressure is set by cavity pressure at gate freeze, not by a number on the controller. How to find gate freeze and what happens either side of it.","_seopress_robots_index":"","_seopress_robots_follow":"","_seopress_robots_imageindex":"","_seopress_robots_snippet":"","_seopress_robots_primary_cat":"35","_seopress_robots_breadcrumbs":"","_seopress_robots_freeze_modified_date":"","_seopress_robots_custom_modified_date":"","_seopress_robots_canonical":"","_seopress_social_fb_title":"","_seopress_social_fb_desc":"","_seopress_social_fb_img":"","_seopress_social_fb_img_attachment_id":0,"_seopress_social_fb_img_width":0,"_seopress_social_fb_img_height":0,"_seopress_social_twitter_title":"","_seopress_social_twitter_desc":"","_seopress_social_twitter_img":"","_seopress_social_twitter_img_attachment_id":0,"_seopress_social_twitter_img_width":0,"_seopress_social_twitter_img_height":0,"_seopress_redirections_value":"","_seopress_redirections_enabled":"","_seopress_redirections_enabled_regex":"","_seopress_redirections_logged_status":"","_seopress_redirections_param":"","_seopress_redirections_type":0,"_seopress_analysis_target_kw":"packing pressure hold time","footnotes":""},"categories":[35],"tags":[],"class_list":["post-7679","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-injection-molding"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/posts\/7679","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/comments?post=7679"}],"version-history":[{"count":0,"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/posts\/7679\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/media\/7672"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/media?parent=7679"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/categories?post=7679"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/fr\/wp-json\/wp\/v2\/tags?post=7679"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}