{"id":7758,"date":"2025-09-17T09:00:00","date_gmt":"2025-09-17T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/plug-assist-thin-gauge-forming\/"},"modified":"2025-09-17T09:00:00","modified_gmt":"2025-09-17T08:00:00","slug":"plug-assist-thin-gauge-forming","status":"publish","type":"post","link":"https:\/\/uplastech.com\/es\/plug-assist-thin-gauge-forming\/","title":{"rendered":"Plug Assist in Thin-Gauge Thermoforming: Prestretch and Wall Profile"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/plug-assist-thin-gauge-forming.jpg\" alt=\"Synthetic plug assist tool above a thin-gauge thermoforming mould cavity\" width=\"1536\" height=\"909\"><figcaption>A plug does not push the sheet into the mould. It pre-stretches it so that the vacuum has less work to do, and the wall profile changes completely.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"vacuum\">What vacuum alone does to a wall<\/h2>\n<p>Vacuum forming pulls the sheet into the mould. On a shallow part that works, because the sheet only has to travel a short distance and the stretch is spread over a large area. On a deep part it fails, and the failure is arithmetic.<\/p>\n<p>Take a cup 100 mm deep and 80 mm across, formed from a 1.0 mm sheet with vacuum alone. The base of the cup is the last part of the sheet to enter the mould and the first part to be stretched, and it is stretched against nothing. By the time the base reaches the bottom of the cavity, the material that started at 1.0 mm has been drawn down to 0.15 to 0.25 mm.<\/p>\n<p>That is a 75 to 85% reduction, and it produces a part with a base so thin it flexes under its own contents, a barrier layer that is no longer continuous, and a bottom corner that cracks on demould.<\/p>\n<table>\n<thead>\n<tr>\n<th>Position on the part<\/th>\n<th>Vacuum only<\/th>\n<th>With plug assist<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Base centre<\/td>\n<td>15 \u2013 25% of original<\/td>\n<td>40 \u2013 60% of original<\/td>\n<\/tr>\n<tr>\n<td>Base corner<\/td>\n<td>20 \u2013 30%<\/td>\n<td>45 \u2013 60%<\/td>\n<\/tr>\n<tr>\n<td>Lower side wall<\/td>\n<td>55 \u2013 70%<\/td>\n<td>45 \u2013 60%<\/td>\n<\/tr>\n<tr>\n<td>Upper side wall<\/td>\n<td>85 \u2013 95%<\/td>\n<td>80 \u2013 90%<\/td>\n<\/tr>\n<tr>\n<td>Rim<\/td>\n<td>95 \u2013 100%<\/td>\n<td>95 \u2013 100%<\/td>\n<\/tr>\n<tr>\n<td>Range across the part<\/td>\n<td>5 : 1<\/td>\n<td>2 : 1<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 Wall distribution with and without plug assist, 100 mm cup from 1.0 mm sheet. The range is what matters, not the absolute values.<\/p>\n<p>The last row is the real argument. A wall that varies from 0.15 to 1.0 mm is a part with a weak point that decides everything else: the load it can carry, the drop height it survives, the barrier it provides, the weight it can be specified at. A wall that varies from 0.45 to 1.0 mm is a part that can be engineered.<\/p>\n<h2 id=\"how\">How plug assist changes the profile<\/h2>\n<p>A plug is a male tool that descends into the sheet before the vacuum is applied. It does two things at once, and they act in opposite directions, which is why the setup is a balance rather than a maximum.<\/p>\n<p><strong>It pre-stretches mechanically.<\/strong> The plug pushes the centre of the sheet down into the cavity, so the material that will become the base is stretched against the plug face rather than against air. Because the plug is a solid surface, the stretch is distributed over the whole contact area instead of concentrating at the base corner.<\/p>\n<p><strong>It chills the contact area.<\/strong> The plug is cooler than the sheet, so the material that touches it solidifies slightly and resists further thinning. That is what stops the base from drawing down to nothing \u2014 but it also means the contact area ends up thinner than the material immediately around it, because the chilled material cannot flow to relieve the stretch.<\/p>\n<p>The result is a characteristic thickness profile: thin at the point of plug contact, thicker in a ring around it, then thinning again down the side wall. A well-set plug makes that profile gentle. A badly set one makes it a step.<\/p>\n<div class=\"callout\">\n<p><strong>The plug trades one thin spot for another, and it trades a bad one for a good one.<\/strong> Without a plug the thin spot is the base corner, which is where a part fails. With a plug it is the base centre, which is usually the least critical area.<\/p>\n<\/div>\n<h2 id=\"material\">Plug material: the four options<\/h2>\n<p>Plug material is chosen for its thermal conductivity, its machinability and its friction against hot plastic. Those three properties point at four different answers.<\/p>\n<table>\n<thead>\n<tr>\n<th>Material<\/th>\n<th>Conductivity<\/th>\n<th>Coste<\/th>\n<th>Lo mejor para<\/th>\n<th>Weakness<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Synthetic (epoxy + glass microspheres)<\/td>\n<td>0.2 \u2013 0.4 W\/m\u00b7K<\/td>\n<td>Medio<\/td>\n<td>Most thin-gauge work<\/td>\n<td>Chips at edges, cannot be repaired<\/td>\n<\/tr>\n<tr>\n<td>Hardwood (maple, beech)<\/td>\n<td>0.15 W\/m\u00b7K<\/td>\n<td>Bajo<\/td>\n<td>Prototypes, short runs<\/td>\n<td>Absorbs moisture, changes size, short life<\/td>\n<\/tr>\n<tr>\n<td>Aluminium<\/td>\n<td>200 W\/m\u00b7K<\/td>\n<td>Alta<\/td>\n<td>High-temperature materials, long runs<\/td>\n<td>Must be heated or it chills the sheet<\/td>\n<\/tr>\n<tr>\n<td>PTFE or coated<\/td>\n<td>0.25 W\/m\u00b7K<\/td>\n<td>Medio<\/td>\n<td>Sticky materials, PET, PS<\/td>\n<td>Soft, wears, expensive to resurface<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 Plug materials. The conductivity column explains why aluminium only works when it is heated.<\/p>\n<p>Synthetic material \u2014 an epoxy or polyurethane loaded with hollow glass microspheres \u2014 is the default for thin-gauge work. Its low conductivity means it does not chill the sheet on contact, it machines like hardwood, and it can be shaped to almost any profile. The limitation is that it is brittle at thin sections, so plug edges chip and the chips cannot be filled.<\/p>\n<p>Hardwood is the cheapest option and it works well for a trial. It absorbs moisture from the air and from the sheet, which changes its dimensions by a few tenths of a millimetre over a week, and that is enough to change the wall profile. A wooden plug is a prototype tool, not a production one.<\/p>\n<p>Aluminium is the opposite problem. Its conductivity is 500 times that of the synthetic material, so an unheated aluminium plug chills the sheet on contact and produces a hard, thin, glossy patch that will not stretch. An aluminium plug has to be heated to within 20 to 40 \u00b0C of the sheet temperature to behave, and at that point it is a hot tool with all the plumbing that implies.<\/p>\n<p>PTFE and PTFE-coated plugs are used where the material sticks. PET at forming temperature is tacky, and a bare plug will drag and leave marks. A PTFE surface eliminates that, at the cost of a soft surface that wears and needs periodic replacement.<\/p>\n<h2 id=\"temp\">Plug temperature is the real control<\/h2>\n<p>Most plug problems are temperature problems, and the direction of the error decides the defect.<\/p>\n<table>\n<thead>\n<tr>\n<th>Plug temperature<\/th>\n<th>What happens<\/th>\n<th>Wall profile<\/th>\n<th>Surface<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Cold, under 50 \u00b0C<\/td>\n<td>Contact area freezes instantly<\/td>\n<td>Very thin at contact, thick ring around it<\/td>\n<td>Dull, may show chill marks<\/td>\n<\/tr>\n<tr>\n<td>Warm, 60 \u2013 100 \u00b0C<\/td>\n<td>Balanced<\/td>\n<td>Gentle gradient<\/td>\n<td>Bien<\/td>\n<\/tr>\n<tr>\n<td>Hot, over 120 \u00b0C<\/td>\n<td>Material sticks and drags<\/td>\n<td>Thin and uneven<\/td>\n<td>Glossy, may pick up plug marks<\/td>\n<\/tr>\n<tr>\n<td>Same as sheet<\/td>\n<td>No chilling at all<\/td>\n<td>Thinnest possible base<\/td>\n<td>Excelente<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 \u2014 Plug temperature against result. \"Same as sheet\" is a real technique for surface-critical parts, at the cost of base thickness.<\/p>\n<p>The counter-intuitive row is the last one. A plug held at the same temperature as the sheet does not chill anything, so the material flows freely around it and the base ends up thinner than with a warm plug. What it buys is surface quality: no chill marks, no drag, no matte patch where the plug touched. For a cosmetic part that is the right trade; for a structural tray it is not.<\/p>\n<p>The practical target for most thin-gauge work is 60 to 100 \u00b0C, achieved by a cartridge heater in the plug body with a thermocouple. A plug without temperature control is a plug running at whatever the shop is, which in winter is 18 \u00b0C and in summer is 35 \u00b0C, and the wall profile changes with the season.<\/p>\n<h2 id=\"geometry\">Geometry: size, radius, shape<\/h2>\n<p>Plug geometry is set by three numbers, and each has a range rather than a value.<\/p>\n<p><strong>Clearance to the cavity wall.<\/strong> The plug has to be smaller than the cavity by enough to let the sheet pass, which means the sheet thickness plus a margin. Too little and the sheet is trapped and tears; too much and the plug does not prestretch the side wall at all. For a 1 mm sheet the radial clearance is typically 1.5 to 2.5 mm per side.<\/p>\n<p><strong>Base clearance.<\/strong> The plug must not touch the cavity base in normal operation, or it will punch through. A gap of 0.8 to 1.0 times the sheet thickness at the bottom of the stroke is standard, and it is set by the machine's stroke stop rather than by the plug length.<\/p>\n<p><strong>Top radius.<\/strong> A sharp plug top concentrates the stretch and produces a ring of very thin material at the contact edge. The radius should be at least two to four times the sheet thickness, and more for a deep draw.<\/p>\n<table>\n<thead>\n<tr>\n<th>Par\u00e1metro<\/th>\n<th>Typical value<\/th>\n<th>Effect of getting it wrong<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Radial clearance<\/td>\n<td>1.5 \u2013 2.5 mm per side<\/td>\n<td>Too small: tearing. Too large: no side-wall prestretch<\/td>\n<\/tr>\n<tr>\n<td>Base clearance at full stroke<\/td>\n<td>0.8 \u2013 1.0 \u00d7 sheet thickness<\/td>\n<td>Zero: punch-through. Large: no base prestretch<\/td>\n<\/tr>\n<tr>\n<td>Top edge radius<\/td>\n<td>2 \u2013 4 \u00d7 sheet thickness<\/td>\n<td>Sharp: thin ring at the contact edge<\/td>\n<\/tr>\n<tr>\n<td>Side wall draft<\/td>\n<td>2 \u2013 5\u00b0<\/td>\n<td>Zero: drag marks on the side wall<\/td>\n<\/tr>\n<tr>\n<td>Surface finish<\/td>\n<td>Ra 0.8 or better<\/td>\n<td>Rough: visible marks on the inside of the part<\/td>\n<\/tr>\n<tr>\n<td>Plug area \/ cavity area<\/td>\n<td>0.6 \u2013 0.85<\/td>\n<td>Too small: no prestretch. Too large: trapped sheet<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 4 \u2014 Plug geometry. The area ratio is the parameter that best predicts whether the plug is doing its job.<\/p>\n<p>The area ratio is worth calculating because it is the single number that describes how much prestretch the plug provides. A plug whose cross-section is 60% of the cavity area will prestretch the sheet by a factor of about 1.7 before the vacuum does anything. At 85% the factor is 1.2, and the plug is mostly acting as a chill surface rather than a stretcher.<\/p>\n<h2 id=\"setup\">Setting up a plug, step by step<\/h2>\n<p>A plug is not a part you fit and forget. It is a tool that has to be tuned against the wall thickness you want, and the tuning is empirical because the material behaviour is not predictable enough to calculate.<\/p>\n<p><strong>Start with the geometry from Table 4.<\/strong> Cut the plug to the nominal dimensions, machine the top radius generously, and leave the length slightly long so it can be shortened.<\/p>\n<p><strong>Set the stroke so the plug stops short of the base.<\/strong> Bring the plug down by hand with no sheet, measure the gap, and set the machine stop to leave 0.8 to 1.0 times the sheet thickness.<\/p>\n<p><strong>Run one shot and cut the part.<\/strong> Section it through the centre and measure the wall at the base centre, the base corner, and three points up the side wall. That profile is the only data that matters.<\/p>\n<p><strong>Adjust in one direction at a time.<\/strong> A thin base centre means the plug is too cold or too small; a thick base with a thin corner means the plug is too large or the top radius is too sharp. Change one thing, run again, measure again.<\/p>\n<p><strong>Record the settings that worked.<\/strong> Plug temperature, stroke, and the resulting wall profile belong in the tool record. The next person to run the job will not rediscover them.<\/p>\n<h2 id=\"materials\">Which materials need a plug<\/h2>\n<table>\n<thead>\n<tr>\n<th>Material<\/th>\n<th>Plug needed above<\/th>\n<th>Note<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>PP<\/td>\n<td>0.6 : 1<\/td>\n<td>Low melt strength, needs help earliest<\/td>\n<\/tr>\n<tr>\n<td>HIPS<\/td>\n<td>0.7 : 1<\/td>\n<td>Softer than GPPS<\/td>\n<\/tr>\n<tr>\n<td>GPPS<\/td>\n<td>0.8 : 1<\/td>\n<td>Good melt strength, tolerates more draw<\/td>\n<\/tr>\n<tr>\n<td>APET<\/td>\n<td>0.8 : 1<\/td>\n<td>Stiff, but thins fast once it yields<\/td>\n<\/tr>\n<tr>\n<td>CPET<\/td>\n<td>0.9 : 1<\/td>\n<td>Stretches less; the plug is mostly for distribution<\/td>\n<\/tr>\n<tr>\n<td>PVC<\/td>\n<td>0.9 : 1<\/td>\n<td>Good melt strength<\/td>\n<\/tr>\n<tr>\n<td>PMMA<\/td>\n<td>1.0 : 1<\/td>\n<td>Rarely plugged; surface marks are unacceptable<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 5 \u2014 Draw ratio at which each material needs plug assist. PP is the earliest by a clear margin.<\/p>\n<p>The thresholds are rules of thumb and they assume a warm plug. A cold plug effectively raises the threshold because it stiffens the sheet on contact, which is why a cold plug on a PP part at 0.7 to 1 produces a part that looks plugged but still has a thin base.<\/p>\n<h2 id=\"defects\">Defects and what they point at<\/h2>\n<table>\n<thead>\n<tr>\n<th>Defecto<\/th>\n<th>Causa<\/th>\n<th>Fix<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Thin ring at the plug contact edge<\/td>\n<td>Top radius too sharp<\/td>\n<td>Increase the radius to 3\u20134 \u00d7 sheet thickness<\/td>\n<\/tr>\n<tr>\n<td>Base centre too thin<\/td>\n<td>Plug too cold, or too small<\/td>\n<td>Raise plug temperature, increase the area ratio<\/td>\n<\/tr>\n<tr>\n<td>Torn sheet at the plug edge<\/td>\n<td>Clearance too tight, or stroke too deep<\/td>\n<td>Open the radial clearance, shorten the stroke<\/td>\n<\/tr>\n<tr>\n<td>Drag marks on the side wall<\/td>\n<td>No draft, or a sticky material<\/td>\n<td>Add 2\u20135\u00b0 draft, PTFE coat the plug<\/td>\n<\/tr>\n<tr>\n<td>Matte patch where the plug touched<\/td>\n<td>Plug too cold<\/td>\n<td>Raise temperature, or accept for non-cosmetic parts<\/td>\n<\/tr>\n<tr>\n<td>Webbing still present<\/td>\n<td>Plug does not prestretch the corners<\/td>\n<td>Reshape the plug to match the cavity corners<\/td>\n<\/tr>\n<tr>\n<td>Wall varies shot to shot<\/td>\n<td>Plug temperature drifting<\/td>\n<td>Add thermocouple control, not just a heater<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 6 \u2014 Plug defects. The last row is the most common and the cheapest to fix.<\/p>\n<p>Webbing is the one that a plug sometimes fails to solve. Webbing happens when the sheet folds between two deep cavities before it can be drawn into either, and it is caused by the sheet being too hot, too slack, or the cavity spacing being too tight. A plug helps because it takes up the slack, but if the web area is too narrow no plug will fix it and the cavity layout has to change.<\/p>\n<div class=\"faq\">\n<h3>What does plug assist actually do?<\/h3>\n<p>It mechanically pre-stretches the sheet before the vacuum is applied, so the base is stretched against a solid surface instead of against air. It also chills the contact area, which resists further thinning.<\/p>\n<h3>When do I need plug assist?<\/h3>\n<p>Above a draw ratio of roughly 0.6 to 1 for PP, 0.8 to 1 for PS and APET, and 0.9 to 1 for CPET. Below those ratios vacuum alone gives an acceptable wall.<\/p>\n<h3>What is the best plug material?<\/h3>\n<p>Synthetic epoxy loaded with glass microspheres for most thin-gauge work. Aluminium only if it is heated, hardwood only for prototypes, PTFE where the material sticks.<\/p>\n<h3>What temperature should a plug run at?<\/h3>\n<p>60 to 100 \u00b0C for a balanced wall profile. Below 50 \u00b0C the contact area freezes and the base thins; above 120 \u00b0C the material drags and sticks.<\/p>\n<h3>How much clearance between plug and cavity?<\/h3>\n<p>1.5 to 2.5 mm per side for a 1 mm sheet, plus 0.8 to 1.0 times the sheet thickness at the base of the stroke. Too little tears the sheet, too much removes the side-wall prestretch.<\/p>\n<h3>Why is my base still thin with a plug?<\/h3>\n<p>The plug is too cold, too small, or stops too far from the base. A cold plug freezes the contact area before it can stretch, and a small plug does not prestretch enough.<\/p>\n<h3>Does a plug always improve the wall?<\/h3>\n<p>It improves the base and the lower side wall, and it makes the base centre slightly thinner than the surrounding ring. It is a trade, and it is almost always a good one because the base corner is where parts fail.<\/p>\n<h3>Can I use one plug for several cavity shapes?<\/h3>\n<p>Only if the cavities are the same shape. A plug is matched to the cavity profile; using one plug across different shapes gives uneven prestretch and unpredictable walls.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Getting a thin base on a deep draw?<\/p>\n<p>Send the cavity drawing and the sheet thickness. We will tell you whether a plug is needed, what area ratio to aim for, and what wall profile the part can realistically hold.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/es\/custom-vacuum-forming\/\">Talk to a thin-gauge thermoforming engineer<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/es\/pp-thin-gauge-thermoforming\/\">PP Thin-Gauge Thermoforming: Shrinkage and Warpage<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/es\/vacuum-forming-wall-thickness\/\">Vacuum Forming Wall Thickness: Draw Ratio and Thinning<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/es\/como-evitar-la-formacion-de-bandas-en-el-termoconformado-una-guia-completa\/\">How to Prevent Webbing in Thermoforming<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/es\/vacuum-forming-mold-design\/\">Vacuum Forming Mold Design<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/es\/form-cut-stack-inline-thermoforming\/\">Form-Cut-Stack: How an Inline Line Runs<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Vacuum alone draws a 1 mm sheet down to 0.2 mm at the base corner. What a plug does, the four plug materials, and why temperature decides the wall profile.<\/p>","protected":false},"author":1,"featured_media":7751,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_seopress_titles_title":"Plug Assist in Thin-Gauge Thermoforming: Prestretch and Wall","_seopress_titles_desc":"Vacuum alone draws a 1 mm sheet down to 0.2 mm at the base corner. What a plug does, the four plug materials, and why temperature decides the wall profile.","_seopress_robots_index":"","_seopress_robots_follow":"","_seopress_robots_imageindex":"","_seopress_robots_snippet":"","_seopress_robots_primary_cat":"29","_seopress_robots_breadcrumbs":"","_seopress_robots_freeze_modified_date":"","_seopress_robots_custom_modified_date":"","_seopress_robots_canonical":"","_seopress_social_fb_title":"","_seopress_social_fb_desc":"","_seopress_social_fb_img":"","_seopress_social_fb_img_attachment_id":0,"_seopress_social_fb_img_width":0,"_seopress_social_fb_img_height":0,"_seopress_social_twitter_title":"","_seopress_social_twitter_desc":"","_seopress_social_twitter_img":"","_seopress_social_twitter_img_attachment_id":0,"_seopress_social_twitter_img_width":0,"_seopress_social_twitter_img_height":0,"_seopress_redirections_value":"","_seopress_redirections_enabled":"","_seopress_redirections_enabled_regex":"","_seopress_redirections_logged_status":"","_seopress_redirections_param":"","_seopress_redirections_type":0,"_seopress_analysis_target_kw":"plug assist thermoforming","footnotes":""},"categories":[29],"tags":[],"class_list":["post-7758","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-vacuum-forming"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/posts\/7758","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/comments?post=7758"}],"version-history":[{"count":0,"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/posts\/7758\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/media\/7751"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/media?parent=7758"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/categories?post=7758"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/es\/wp-json\/wp\/v2\/tags?post=7758"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}