{"id":7902,"date":"2025-11-16T09:00:00","date_gmt":"2025-11-16T09:00:00","guid":{"rendered":"https:\/\/uplastech.com\/sink-marks-injection-molding\/"},"modified":"2025-11-16T09:00:00","modified_gmt":"2025-11-16T09:00:00","slug":"sink-marks-injection-molding","status":"publish","type":"post","link":"https:\/\/uplastech.com\/de\/sink-marks-injection-molding\/","title":{"rendered":"Sink Marks in Injection Molding: Ribs, Bosses and the Packing That Cannot Reach"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/sink-marks-injection-molding.jpg\" alt=\"Sink depth against rib thickness ratio, and sink depth against distance from the gate\" width=\"1536\" height=\"909\"><figcaption>Sink depth rises steeply once the rib exceeds half the wall, and it grows again with every centimetre the rib sits from the gate.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"what\">What a sink mark actually is<\/h2>\n<p>A sink mark is a shallow depression on the surface of a moulded part, and it is always the same story: a region of the part was still molten and shrinking after the surface skin had frozen solid, and it pulled the skin down with it. The skin is a thin solid shell; underneath it, the core is cooling and contracting; the shell cannot resist the tension, so it deflects inward and stays there.<\/p>\n<p>The amount of contraction is not small. An unfilled polypropylene shrinks 1.5 to 2 percent linearly, which is 4 to 6 percent by volume. A polyamide shrinks more. A 4 mm thick section shrinking 5 percent by volume wants to lose 0.2 mm of thickness, and if the surface is already frozen, that 0.2 mm has to come from somewhere: it comes from the surface moving inward.<\/p>\n<p>This is why sink marks are a thickness problem before they are a process problem. Uniform wall sections cool and shrink uniformly and the shrinkage is taken up by the part getting slightly smaller overall, which is what the mould shrinkage allowance is for. Where the wall is not uniform, the thick region shrinks more than the thin region around it, and the difference has to go somewhere visible.<\/p>\n<h2 id=\"ribs\">Ribs, bosses and the half-wall rule<\/h2>\n<p>A rib is a thick section attached to a thin wall, and it is the most common source of sink marks in the industry. The rule that every designer is taught is that a rib should be no thicker than half the adjoining wall, and like most rules of thumb it is approximately right for a reason that can be quantified.<\/p>\n<p>At a rib-to-wall ratio of 0.4 the sink is 2 microns, which is invisible. At 0.5 it is 6 microns, which is invisible on a textured surface and barely detectable on a polished one. At 0.6 it is 15 microns, which shows as a faint line on a gloss surface. At 0.8 it is 38 microns and at 1.0 it is 62 microns, and at that point the mark is obvious from a metre away.<\/p>\n<table>\n<thead>\n<tr>\n<th>Rib \/ wall ratio<\/th>\n<th>Sink depth, um<\/th>\n<th>Stiffness gained<\/th>\n<th>Verdict<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>0.4<\/td>\n<td>2<\/td>\n<td>About 40 percent of a full-thickness rib<\/td>\n<td>Invisible; use this where cosmetics matter<\/td>\n<\/tr>\n<tr>\n<td>0.5<\/td>\n<td>6<\/td>\n<td>About 50 percent<\/td>\n<td>The practical limit for a visible surface<\/td>\n<\/tr>\n<tr>\n<td>0.6<\/td>\n<td>15<\/td>\n<td>About 60 percent<\/td>\n<td>Acceptable on a textured or hidden face<\/td>\n<\/tr>\n<tr>\n<td>0.8<\/td>\n<td>38<\/td>\n<td>About 80 percent<\/td>\n<td>Visible; needs a process fix or a cosmetic cover<\/td>\n<\/tr>\n<tr>\n<td>1.0<\/td>\n<td>62<\/td>\n<td>100 percent<\/td>\n<td>Obvious; redesign the rib or move the surface<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 Rib thickness against sink depth and the stiffness it buys.<\/p>\n<p>The stiffness column is what makes the rule painful, because it shows what is being given up. A rib at half the wall gives roughly half the stiffness of a full-thickness rib, so following the rule costs real performance. The way out is not to thicken the rib but to add more of them: two ribs at 0.5 give more stiffness than one rib at 1.0, and neither of them sinks.<\/p>\n<h2 id=\"packing\">Why packing cannot reach a distant rib<\/h2>\n<p>The instinctive fix for a sink mark is more packing pressure, and it works when the sink is near the gate and fails when it is not. The reason is that packing only helps while the gate is open and the cavity is hydraulically connected. Once the gate freezes, the part is a sealed volume, and pressure applied at the sprue does nothing at all inside it.<\/p>\n<p>Even before the gate freezes, pressure decays along the flow path. The melt is viscous, the channel is thin, and the pressure drop from gate to the far end of a 250 mm part is substantial. Measured sink depth against distance from the gate runs 8 microns at 50 mm, 14 at 100, 22 at 150, 32 at 200 and 45 at 250. The far end of the part is effectively unpacked even when the near end is fully packed.<\/p>\n<p>There are three consequences. A sink near the gate is a packing problem and can be fixed with pressure and hold time. A sink far from the gate is a gate position problem and can only be fixed by moving the gate, adding a second gate, or thickening the feed path. And a sink that appears only on the far cavity of a multi-cavity tool is a runner balance problem, because the far cavity is seeing a lower pressure for the whole of the pack phase.<\/p>\n<div class=\"callout\">Before increasing packing pressure, check where the sink is. If it is more than about 150 mm from the gate, the pressure is not arriving and raising it will only add stress near the sprue.<\/div>\n<h2 id=\"fixes\">The three fixes that work<\/h2>\n<p>Every real fix falls into one of three families, and they are worth considering in this order because the cost rises sharply from one to the next.<\/p>\n<table>\n<thead>\n<tr>\n<th>Fix<\/th>\n<th>What it does<\/th>\n<th>Kosten<\/th>\n<th>When to use it<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Geometry: core the rib or thin it to 0.5<\/td>\n<td>Removes the thick section, so there is no differential shrinkage<\/td>\n<td>Free at the design stage; a tool change later<\/td>\n<td>Always the first choice, and almost always sufficient<\/td>\n<\/tr>\n<tr>\n<td>Gate: move it, add one, or enlarge it<\/td>\n<td>Gets packing pressure to the region that needs it<\/td>\n<td>A tool modification, days of downtime<\/td>\n<td>When the sink is far from the gate and the geometry cannot change<\/td>\n<\/tr>\n<tr>\n<td>Process: pack pressure, hold time, melt temperature<\/td>\n<td>Packs more material in while the gate is open<\/td>\n<td>Free, but limited by flash and stress<\/td>\n<td>When the sink is close to the gate and the gate is large<\/td>\n<\/tr>\n<tr>\n<td>Material: lower shrinkage grade or a foaming agent<\/td>\n<td>Reduces volumetric shrinkage or offsets it with gas<\/td>\n<td>A material change and a re-validation<\/td>\n<td>When geometry and gate are both fixed<\/td>\n<\/tr>\n<tr>\n<td>Cosmetics: texture the surface<\/td>\n<td>Hides a shallow sink without removing it<\/td>\n<td>A tool texture, one-off<\/td>\n<td>When the sink is 10 to 20 microns and the part is not optical<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 The fixes, in the order they should be considered.<\/p>\n<p>The texture option deserves a note because it is used more than it is admitted. A matte texture with a depth of 20 to 30 microns will hide a sink of 10 microns completely, and it is a legitimate engineering answer when the alternative is a tool change. What it is not is an answer for a 60 micron sink, which will still read as a glossy patch inside the matte field.<\/p>\n<h2 id=\"bosses\">Bosses are worse than ribs<\/h2>\n<p>A boss is a cylindrical feature, usually around a screw hole, and it is worse than a rib for a simple geometric reason: the wall thickness at the base of a boss is the full diameter of the boss, not the wall of the tube. A boss 8 mm outside diameter with a 4 mm hole has a 2 mm wall, but where it meets a 2 mm plate the local section is 8 mm of material with a hole in it, and that is four times the plate thickness.<\/p>\n<p>The standard mitigations are all geometric. Core the boss from the back if the design allows. Use a boss with a wall of 0.6 times the plate rather than a solid cylinder. Add gussets, which spread the section change over a longer distance and reduce the concentration. And keep the boss short, because a tall boss has more mass and shrinks more.<\/p>\n<p>There is a process trick that works on bosses better than on ribs: core the boss out with a moving core or a secondary operation, so that the moulded feature is a tube rather than a cylinder. A tube of 2 mm wall on a 2 mm plate sinks almost not at all, and the hole is drilled afterwards. The cost is a secondary operation, and it is often cheaper than the sink mark.<\/p>\n<div class=\"myth\">A boss is fine as long as the wall is thin. The boss wall being thin does not help, because the sink is caused by the mass at the base where the boss meets the plate, and that mass is the diameter, not the wall.<\/div>\n<h2 id=\"sink-void\">Sink against void: the same cause, two symptoms<\/h2>\n<p>The same shrinkage that produces a visible sink mark can instead produce an internal void, and which one you get depends on how stiff the surface is relative to the pull of the shrinking core. A part with a strong, thick, cool skin pulls the surface in and shows a sink. A part with a hot, weak skin lets the core pull away from the skin and creates a void inside the thick section, with a perfectly good surface.<\/p>\n<p>This matters because the two are confused constantly. A part that passes a visual inspection and fails a mechanical test may be full of voids. The way to tell is to cut the part through the suspect section: a sink shows as a depression on the surface with sound material behind it, and a void shows as a cavity inside with a surface that looks fine.<\/p>\n<table>\n<thead>\n<tr>\n<th>Symptom<\/th>\n<th>Where it shows<\/th>\n<th>What is happening<\/th>\n<th>Fix<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Sink mark<\/td>\n<td>Surface depression above a rib or boss<\/td>\n<td>The skin is stiff enough to be pulled in<\/td>\n<td>Thin the section, pack harder, move the gate<\/td>\n<\/tr>\n<tr>\n<td>Internal void<\/td>\n<td>Nothing visible; found by cutting or X-ray<\/td>\n<td>The skin is too weak to follow the core<\/td>\n<td>Raise pack pressure and hold time, lower melt temperature<\/td>\n<\/tr>\n<tr>\n<td>Warp<\/td>\n<td>Part bows after ejection<\/td>\n<td>Differential shrinkage across the part<\/td>\n<td>Balance cooling, equalise wall, add a fixture<\/td>\n<\/tr>\n<tr>\n<td>Gloss difference<\/td>\n<td>Shiny patch in a matte field<\/td>\n<td>A shallow sink that has changed the surface topography<\/td>\n<td>Texture depth, or thin the section<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 \u2014 Four symptoms of the same shrinkage, and how to tell them apart.<\/p>\n<h2 id=\"rules\">Design rules that avoid it<\/h2>\n<p>Sink marks are almost entirely a design outcome. A part designed with uniform wall, ribs at half the wall and cored bosses will not sink even on a mediocre process. A part designed with a 4 mm rib on a 2 mm wall will sink on the best process in the building.<\/p>\n<ol>\n<li>Keep the nominal wall as uniform as the function allows, and transition thickness gradually rather than in a step.<\/li>\n<li>Ribs at 0.5 to 0.6 of the wall, and use more ribs rather than thicker ones to recover stiffness.<\/li>\n<li>Bosses cored to a wall of 0.6 of the plate, with gussets, and kept as short as the screw length allows.<\/li>\n<li>Put the gate where the thickest section is, so that packing reaches the mass before the gate freezes.<\/li>\n<li>Avoid thick corners where two walls meet; a radius is better than a sharp corner, and a cored corner is better than either.<\/li>\n<li>If the surface must be cosmetic, specify the texture before the tool is cut, not after the first samples sink.<\/li>\n<\/ol>\n<p>The last point is the one that saves the most money. A texture specification written into the tool drawing costs nothing. A texture added to an existing tool costs a re-polish and a re-texture, and if the sink is deep it will not fix it anyway.<\/p>\n<div class=\"faq\">\n<h3>Why does more packing pressure not fix my sink mark?<\/h3>\n<p>Because the sink is probably further from the gate than the pressure can reach. Once the gate freezes the part is a sealed volume, and pressure at the sprue does nothing. Sink beyond about 150 mm from the gate is a gate position problem.<\/p>\n<h3>What is the maximum rib thickness to avoid sink?<\/h3>\n<p>Half the adjoining wall for a visible surface, and 0.6 for a hidden or textured one. At 0.8 the sink is around 38 microns and is visible on gloss; at 1.0 it is over 60.<\/p>\n<h3>Are bosses worse than ribs for sink?<\/h3>\n<p>Yes, because the section at the base of a boss is its full diameter, not its wall. A boss with a 2 mm wall on a 2 mm plate still has an 8 mm mass where it meets the plate.<\/p>\n<h3>How do I tell a sink from a void?<\/h3>\n<p>Cut the part through the suspect section. A sink is a surface depression with sound material behind it; a void is an internal cavity with an intact surface. Both come from the same shrinkage.<\/p>\n<h3>Can a texture hide a sink mark?<\/h3>\n<p>Up to about 10 to 15 microns, yes. Beyond that the sink reads as a glossy patch inside the matte field and is often more obvious than it was on a smooth surface.<\/p>\n<h3>Why does only one cavity of my tool sink?<\/h3>\n<p>Runner imbalance. The far cavity sees a lower pressure for the whole pack phase, so it is effectively under-packed even when the near cavity is correct. Balance the runner before changing the process.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Chasing a sink mark on a cosmetic part?<\/p>\n<p>Send the wall section and the rib or boss geometry. We will tell you whether the section can be cored, what rib ratio your stiffness target allows, and whether the gate is in the right place.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/de\/custom-injection-molding\/\">Talk to an injection molding engineer<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/de\/injection-molding-design-guidelines\/\">Injection Molding Design Guidelines: 12 Rules That Cut Part Cost<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/de\/packing-pressure-hold-time\/\">Packing Pressure and Hold Time: How to Set Them From the Part<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/de\/injection-molding-cooling-time\/\">Cooling Time in Injection Molding: The Calculation That Sets Cycle Time<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/de\/injection-molding-defects\/\">Injection Molding Defects: 12 Problems, Their Causes and Fixes<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/de\/clamping-force-tonnage-selection\/\">Clamping Force and Tonnage Selection: The Five-Step Calculation<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>A sink mark is a shrinkage problem that happens after the gate has frozen. Below a rib-to-wall ratio of 0.5 it is invisible; at 1.0 it is 62 microns deep, and no packing pressure will reach it.<\/p>","protected":false},"author":1,"featured_media":7901,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[35],"tags":[],"class_list":["post-7902","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-injection-molding"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/posts\/7902","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/comments?post=7902"}],"version-history":[{"count":0,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/posts\/7902\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/media\/7901"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/media?parent=7902"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/categories?post=7902"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/tags?post=7902"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}