{"id":7701,"date":"2025-08-26T09:00:00","date_gmt":"2025-08-26T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/solid-rod-profile-extrusion\/"},"modified":"2025-08-26T09:00:00","modified_gmt":"2025-08-26T08:00:00","slug":"solid-rod-profile-extrusion","status":"publish","type":"post","link":"https:\/\/uplastech.com\/de\/solid-rod-profile-extrusion\/","title":{"rendered":"Solid Rod Profile Extrusion: Cooling, Die Swell and Internal Voids"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u81ea\u52a8\u5c55\u5f00\u7684\u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/solid-rod-profile-extrusion.jpg\" alt=\"Solid plastic rod emerging from an extrusion die into a water cooling trough on an industrial line\" width=\"1536\" height=\"909\"><figcaption>Solid rod looks like the simplest profile there is. It is the one where cooling, die swell and internal shrinkage all conspire at once.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"why\">Why solid rod is harder than it looks<\/h2>\n<p>A round rod has no corners, no thin walls and no difficult flow paths. On paper it should be the easiest thing an extruder makes. In practice it is one of the harder products to hold to tolerance, because every one of its problems is a volume problem rather than a shape problem.<\/p>\n<p>A 40 mm rod has a surface area of 0.126 m\u00b2 per metre of length and a volume of 1.26 litres. That ratio \u2014 ten times worse than a 4 mm wall tube \u2014 is the whole story. Heat has to leave through a small skin, and the core stays molten long after the outside is hard.<\/p>\n<div class=\"callout\">\n<p><strong>The core is the product.<\/strong> A rod that is dimensionally perfect when it leaves the tank can still crack, void or ovalise two days later, because the centre was never actually solid. Cooling to the core, not to the surface, is the specification.<\/p>\n<\/div>\n<h2 id=\"line\">The line, step by step<\/h2>\n<table>\n<thead>\n<tr>\n<th>Stage<\/th>\n<th>What it does<\/th>\n<th>Where it goes wrong<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Die<\/td>\n<td>Forms the melt into a rod of larger diameter than the finished size<\/td>\n<td>Die swell not accounted for; land too short<\/td>\n<\/tr>\n<tr>\n<td>Sizing sleeve<\/td>\n<td>Draws the rod down to final diameter under vacuum<\/td>\n<td>Vacuum too high; slot marks; wear<\/td>\n<\/tr>\n<tr>\n<td>First tank<\/td>\n<td>Sets the skin and locks the diameter<\/td>\n<td>Water too warm; turbulence marks<\/td>\n<\/tr>\n<tr>\n<td>Second tank<\/td>\n<td>Cools the core through to solid<\/td>\n<td>Tank too short; still hot at the cutter<\/td>\n<\/tr>\n<tr>\n<td>Haul-off<\/td>\n<td>Pulls at constant speed and sets the drawdown ratio<\/td>\n<td>Belt slip; uneven pressure on soft rod<\/td>\n<\/tr>\n<tr>\n<td>Cutter<\/td>\n<td>Cuts to length<\/td>\n<td>Clamp crushing; length drift with speed<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 The rod line. The two-tank arrangement is not optional above about 25 mm; one tank cannot remove the heat from the core in the distance available.<\/p>\n<p>Small rod \u2014 under 12 mm \u2014 is often run without a sizing sleeve at all, straight from the die into a water bath with the haul-off setting the diameter by drawdown. That works because the surface-to-volume ratio is high enough for the rod to freeze quickly. Above 20 mm the free-extrusion approach loses control of diameter and the sleeve becomes necessary.<\/p>\n<h2 id=\"cooling\">Cooling a cylinder is a different problem<\/h2>\n<p>Cooling time scales with the square of the characteristic dimension, exactly as it does for a flat sheet, but the constant is different because heat is converging on an axis rather than a plane. For a cylinder cooled from all sides, the practical rule is that the time to solidify the core is roughly proportional to the square of the diameter.<\/p>\n<table>\n<thead>\n<tr>\n<th>Rod diameter<\/th>\n<th>Water bath length needed<\/th>\n<th>Throughput at 3 m\/min<\/th>\n<th>Core solid at cutter?<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>10 mm<\/td>\n<td>3 \u2013 5 m<\/td>\n<td>~20 kg\/h<\/td>\n<td>Ja<\/td>\n<\/tr>\n<tr>\n<td>20 mm<\/td>\n<td>8 \u2013 12 m<\/td>\n<td>~80 kg\/h<\/td>\n<td>Yes, with two tanks<\/td>\n<\/tr>\n<tr>\n<td>30 mm<\/td>\n<td>18 \u2013 25 m<\/td>\n<td>~180 kg\/h<\/td>\n<td>Marginal<\/td>\n<\/tr>\n<tr>\n<td>40 mm<\/td>\n<td>30 \u2013 45 m<\/td>\n<td>~320 kg\/h<\/td>\n<td>No \u2014 needs spray or extended tank<\/td>\n<\/tr>\n<tr>\n<td>60 mm<\/td>\n<td>60 \u2013 90 m<\/td>\n<td>~720 kg\/h<\/td>\n<td>No \u2014 line speed must drop<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 Bath length and throughput for PVC rod at 3 m\/min line speed. The bath length grows faster than the diameter, which is why large rod lines are long and slow.<\/p>\n<p>The practical consequence is that large rod cannot be run at the same line speed as small rod. Trying to do so produces a rod that is hard on the outside and liquid in the middle, and the internal shrinkage that follows shows up as a void, an oval section or a lengthwise crack discovered by the customer.<\/p>\n<p>Spray cooling between tanks helps because it removes the insulating film of still water that builds up around a hot rod. A rod sitting in a tank develops a boundary layer of warm water that travels with it; spray breaks that layer and can double the heat transfer coefficient on the surface for very little capital cost.<\/p>\n<h2 id=\"swell\">Die swell and the sizing decision<\/h2>\n<p>Every melt expands as it leaves the die. For rod the swell is larger than for a thin profile because the die land is short relative to the diameter and there is no calibration surface to restrain it.<\/p>\n<table>\n<thead>\n<tr>\n<th>Material<\/th>\n<th>Typical die swell<\/th>\n<th>Sizing method<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Rigid PVC<\/td>\n<td>10 \u2013 30%<\/td>\n<td>Vacuum sleeve<\/td>\n<\/tr>\n<tr>\n<td>Flexible PVC<\/td>\n<td>20 \u2013 40%<\/td>\n<td>Vacuum sleeve, low vacuum<\/td>\n<\/tr>\n<tr>\n<td>HDPE<\/td>\n<td>40 \u2013 70%<\/td>\n<td>Vacuum sleeve, long taper<\/td>\n<\/tr>\n<tr>\n<td>PP<\/td>\n<td>30 \u2013 50%<\/td>\n<td>Vacuum sleeve<\/td>\n<\/tr>\n<tr>\n<td>ABS<\/td>\n<td>10 \u2013 25%<\/td>\n<td>Vacuum sleeve<\/td>\n<\/tr>\n<tr>\n<td>PC<\/td>\n<td>5 \u2013 15%<\/td>\n<td>Free extrusion or light sleeve<\/td>\n<\/tr>\n<tr>\n<td>Acryl (PMMA)<\/td>\n<td>5 \u2013 20%<\/td>\n<td>Free extrusion into water<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 \u2014 Die swell by material. The die diameter has to be sized for the swell at the running melt temperature, not at a nominal value from a table.<\/p>\n<p>Because swell depends on melt temperature, shear rate and land length, the die has to be trimmed on the actual line at the actual running conditions. A die that produces a 20.0 mm rod at 180 \u00b0C will not produce 20.0 mm at 195 \u00b0C. This is why rod dies are usually supplied with a slightly oversized orifice and finished by the processor.<\/p>\n<p>The drawdown ratio between die and finished rod is the second control. Pulling a rod down hard from a large die gives good concentricity but builds orientation along the axis, which shows up later as lengthwise splitting when the rod is machined or heated. A drawdown of 1.2 to 1.6 is a reasonable compromise; above 2.0 the orientation becomes a liability.<\/p>\n<h2 id=\"straightness\">Straightness: where bend comes from<\/h2>\n<p>Rod bend is almost always a cooling asymmetry, not a die problem. The melt leaves the die at 170\u2013190 \u00b0C and has to be supported until it is stiff enough not to sag. Any asymmetry in that support \u2014 gravity, uneven water flow, a haul-off belt that grips one side harder \u2014 produces a curve.<\/p>\n<table>\n<thead>\n<tr>\n<th>Source of bend<\/th>\n<th>What it looks like<\/th>\n<th>Fix<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Gravity sag before the tank<\/td>\n<td>Consistent bow in one plane, worse on large rod<\/td>\n<td>Shorten the air gap; support with a roller<\/td>\n<\/tr>\n<tr>\n<td>Uneven water flow in the tank<\/td>\n<td>Bow that changes with line speed<\/td>\n<td>Baffles; check inlet position<\/td>\n<\/tr>\n<tr>\n<td>Haul-off belt pressure<\/td>\n<td>Bow plus a flat on one side<\/td>\n<td>Reduce belt pressure; use multi-belt puller<\/td>\n<\/tr>\n<tr>\n<td>Differential cooling top to bottom<\/td>\n<td>Banana shape, concave on the cool side<\/td>\n<td>Rotate the rod in the tank, or spray evenly<\/td>\n<\/tr>\n<tr>\n<td>Sizing sleeve misalignment<\/td>\n<td>Bend plus ovality at the same angular position<\/td>\n<td>Align sleeve to die centre within 0.1 mm<\/td>\n<\/tr>\n<tr>\n<td>Residual stress release after cutting<\/td>\n<td>Straight off the line, bent after a day<\/td>\n<td>Slow the cooling; anneal<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 4 \u2014 Sources of rod bend. The last one is the frustrating case: the rod passes inspection and fails a week later.<\/p>\n<p>The air gap between die and tank is the single most effective lever. Every millimetre of unsupported melt hanging in the air adds sag, and sag on a 40 mm rod at 180 \u00b0C is not small. Getting the tank close to the die \u2014 50\u2013150 mm \u2014 and supporting the rod with a small roller in that gap fixes most bend complaints on large rod before anything else is touched.<\/p>\n<h2 id=\"voids\">Internal voids and the coring problem<\/h2>\n<p>A thick rod cools from the outside in. The skin freezes first and stops moving. The core continues to cool and shrink, but it is now enclosed by a rigid shell, so the shrinkage has to be accommodated by something. What happens is a void: a cavity at or near the centre, sometimes a continuous pipe running the length of the rod.<\/p>\n<table>\n<thead>\n<tr>\n<th>Ursache<\/th>\n<th>Symptom<\/th>\n<th>Countermeasure<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Core shrinkage<\/td>\n<td>Central void, often pear-shaped<\/td>\n<td>Longer cooling; lower melt temperature<\/td>\n<\/tr>\n<tr>\n<td>Moisture in the resin<\/td>\n<td>Many small voids, frothy appearance on a cut face<\/td>\n<td>Dry the resin properly<\/td>\n<\/tr>\n<tr>\n<td>Air entrainment at the die<\/td>\n<td>Bubbles distributed through the section<\/td>\n<td>Check die assembly; reduce screw speed<\/td>\n<\/tr>\n<tr>\n<td>Excessive drawdown<\/td>\n<td>Void elongated along the axis<\/td>\n<td>Reduce drawdown ratio<\/td>\n<\/tr>\n<tr>\n<td>Cooling too fast at the surface<\/td>\n<td>Void close to the skin, off-centre<\/td>\n<td>Graduated cooling; warmer first tank<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 5 \u2014 Voids in solid rod. Distinguishing shrinkage voids from moisture voids takes one cut with a saw: frothy is moisture, smooth-walled and central is shrinkage.<\/p>\n<p>Where the void cannot be eliminated \u2014 very large diameter, fast cycle \u2014 the industry answer is deliberate coring. A small axial hole, 2\u20134 mm, is formed by a pin in the die and gives the shrinking core somewhere to go. The rod is then sold as cored rod, or the hole is plugged. It sounds like a defect and it is standard practice on rod above 50 mm.<\/p>\n<h2 id=\"sections\">Square, hex and special sections<\/h2>\n<p>Non-round solid sections add a corner problem on top of the volume problem. A square rod has four corners that are further from the cooling surface than the faces, so the corners cool last and shrink most. The result is a section that is slightly concave on the faces and rounded at the corners.<\/p>\n<table>\n<thead>\n<tr>\n<th>Section<\/th>\n<th>Main difficulty<\/th>\n<th>Typical tolerance<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Round<\/td>\n<td>Ovality, void, bend<\/td>\n<td>\u00b10.10 mm under 30 mm<\/td>\n<\/tr>\n<tr>\n<td>Square<\/td>\n<td>Concave faces, corner radius drift<\/td>\n<td>\u00b10.15 mm on the across-flats<\/td>\n<\/tr>\n<tr>\n<td>Hexagonal<\/td>\n<td>Unequal across-flats, twist<\/td>\n<td>\u00b10.15 mm across flats<\/td>\n<\/tr>\n<tr>\n<td>Rectangular<\/td>\n<td>Differential cooling across the width<\/td>\n<td>\u00b10.20 mm on thickness<\/td>\n<\/tr>\n<tr>\n<td>D-section<\/td>\n<td>Flat face bow<\/td>\n<td>\u00b10.20 mm on the flat<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 6 \u2014 What is realistically achievable on solid sections. The tolerances are looser than for hollow profile because there is no internal calibration to hold the shape.<\/p>\n<p>The corner radius in the die is the main design lever. A sharp corner in a solid die creates a low-flow region and a stress concentration in the product. Building in a radius of at least 0.5 mm \u2014 more for large sections \u2014 improves both flow and the finished corner. Buyers who specify a sharp corner on a square rod are usually specifying something that will be radiused in practice anyway.<\/p>\n<h2 id=\"tolerance\">Tolerances you can actually hold<\/h2>\n<p>Rod tolerance is a function of diameter and of whether the rod is sized or free-extruded. Free-extruded rod below 10 mm can hold \u00b10.10 mm on a good line; the same rod at 40 mm free-extruded will drift \u00b10.5 mm over a shift. Sizing brings large rod back to \u00b10.15\u20130.25 mm, at the cost of a sleeve that wears.<\/p>\n<p>The measurement itself needs care. A soft rod measured with a micrometer immediately off the line reads small because the material is still warm and compressible. Measure at least 30 minutes after cutting, at 23 \u00b0C, and measure ovality at three positions along a metre rather than at one.<\/p>\n<div class=\"faq\">\n<h3>Why does my rod have a hole down the middle?<\/h3>\n<p>Shrinkage. The skin freezes first, then the core shrinks inside a rigid shell and has nowhere to go. Longer cooling, a lower melt temperature and a graduated first tank all help. Above about 50 mm diameter a deliberate cored hole is normal practice.<\/p>\n<h3>How long does rod need to cool?<\/h3>\n<p>Roughly with the square of the diameter. A 20 mm PVC rod needs 8\u201312 m of tank at 3 m\/min; a 40 mm rod needs 30\u201345 m or a slower line. The test is simple: cut a section and check the centre is not soft.<\/p>\n<h3>Why is my rod bent?<\/h3>\n<p>Almost always asymmetric cooling or an air gap that is too long. Shorten the gap between die and tank, support the rod in that gap, and check that water flow in the tank is even top and bottom. Belt pressure on the haul-off is the second suspect.<\/p>\n<h3>Can I run rod without a sizing sleeve?<\/h3>\n<p>Below about 12 mm, yes \u2014 the haul-off sets the diameter by drawdown and the rod freezes fast enough. Above 20 mm you lose diameter control and the sleeve becomes necessary. Between 12 and 20 mm it depends on the material and the tolerance.<\/p>\n<h3>What die swell should I allow for?<\/h3>\n<p>It depends on the resin: 10\u201330% for rigid PVC, 40\u201370% for HDPE, 5\u201315% for PC. Because swell also depends on melt temperature and shear rate, the die should be trimmed on the actual line at running conditions rather than to a nominal figure.<\/p>\n<h3>Why does my square rod have concave faces?<\/h3>\n<p>The corners cool last and shrink most, pulling the faces in. Increasing the corner radius in the die, slowing the cooling and lowering the melt temperature all reduce it. A small amount of concavity is normal on solid square section.<\/p>\n<h3>How straight can extruded rod be?<\/h3>\n<p>On a well-run line, 1 mm per metre is achievable for rod under 30 mm. Large rod is harder because gravity has more time to act before the skin sets. Straightening after the fact is possible for some materials but it introduces stress.<\/p>\n<h3>Does rod need annealing?<\/h3>\n<p>For machining applications, often yes. Extruded rod carries residual stress from cooling, and machining releases it, producing a bowed part. A tempering cycle at 5\u201310 \u00b0C below the softening point for a few hours removes most of it.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Need solid rod in a difficult section?<\/p>\n<p>Send us the drawing, the resin and the tolerance. We will tell you whether the section is better extruded or machined from stock, and what the die and sizing arrangement would look like.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/de\/losungen-fur-die-kunststoffextrusion\/\">Talk to an extrusion engineer<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/de\/acrylic-rod\/\">Acrylic Rod: Cast vs Extruded and How to Specify It<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/de\/profile-calibration-cooling\/\">Profile Calibration and Cooling: Sizing, Vacuum and Water<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/de\/extrusion-die-design\/\">Extrusion Die Design for Profiles: Flow Balance and Die Swell<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/de\/internal-stress-extruded-profiles\/\">Internal Stress in Extruded Profiles: Annealing and Distortion<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/de\/fehler-in-der-kunststoffextrusion\/\">Plastic Extrusion Defects: 12 Problems, Causes and Fixes<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Solid rod is the hardest simple profile there is. Why the core, not the surface, sets the cooling length \u2014 and where voids and bend actually come from.<\/p>","protected":false},"author":1,"featured_media":7695,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_seopress_titles_title":"Solid Rod Profile Extrusion: Cooling, Die Swell and Internal","_seopress_titles_desc":"Solid rod is the hardest simple profile there is. Why the core, not the surface, sets the cooling length \u2014 and where voids and bend actually come from.","_seopress_robots_index":"","_seopress_robots_follow":"","_seopress_robots_imageindex":"","_seopress_robots_snippet":"","_seopress_robots_primary_cat":"17","_seopress_robots_breadcrumbs":"","_seopress_robots_freeze_modified_date":"","_seopress_robots_custom_modified_date":"","_seopress_robots_canonical":"","_seopress_social_fb_title":"","_seopress_social_fb_desc":"","_seopress_social_fb_img":"","_seopress_social_fb_img_attachment_id":0,"_seopress_social_fb_img_width":0,"_seopress_social_fb_img_height":0,"_seopress_social_twitter_title":"","_seopress_social_twitter_desc":"","_seopress_social_twitter_img":"","_seopress_social_twitter_img_attachment_id":0,"_seopress_social_twitter_img_width":0,"_seopress_social_twitter_img_height":0,"_seopress_redirections_value":"","_seopress_redirections_enabled":"","_seopress_redirections_enabled_regex":"","_seopress_redirections_logged_status":"","_seopress_redirections_param":"","_seopress_redirections_type":0,"_seopress_analysis_target_kw":"solid rod profile extrusion","footnotes":""},"categories":[17],"tags":[],"class_list":["post-7701","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-plastic-extrusion-process"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/posts\/7701","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/comments?post=7701"}],"version-history":[{"count":0,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/posts\/7701\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/media\/7695"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/media?parent=7701"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/categories?post=7701"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/de\/wp-json\/wp\/v2\/tags?post=7701"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}