Silicone Hardness Testing: Shore A, IRHD and the Sample Thickness

A technician in a white coat pressing a Shore A durometer onto a stack of black silicone test slabs on a laboratory bench
The stack is not a habit. Shore A needs at least 6 mm of material under the indentor.

What Shore A actually measures

Shore A measures the resistance of a material to a spring loaded indentor. A truncated cone is pressed into the surface under a defined force, and the depth of penetration is read on a scale from 0 to 100. A soft gel reads near 0, a hard rubber near 100, and a typical silicone gasket sits between 40 and 70.

It is an empirical test, not a material property. The number depends on the geometry of the indentor, the spring rate, the dwell time and the thickness of the sample, and two instruments from different makers can disagree by several points on the same sample. That is why the standard specifies the instrument, the sample and the procedure together, and why a reading without those details is not a measurement.

The scale is also non-linear in terms of modulus. A change from 40 to 50 Shore A is a much larger change in stiffness than a change from 70 to 80, because the indentor geometry and the material response interact differently across the range. Comparing hardness values as if they were linear is a common source of confusion.

For silicone specifically, hardness is set by the filler loading rather than by the polymer. A 40 Shore A compound might have 20 parts of fumed silica per hundred of polymer; a 70 Shore A compound might have 45. That is why hardness and tear strength move together, and why a hardness specification is partly a specification of the filler system.

The thickness problem

The indentor penetrates a finite depth, and the material under it has to be thick enough to behave as if it were infinite. If the sample is thin, the indentor feels the support underneath and reads harder than the material actually is. The standard requires at least 6 mm of material, either as a single slab or as a stack of thinner ones.

The effect is large. The chart on the left shows the same three compounds measured at thicknesses from 1 to 12 mm. At 1 mm, a nominal 80 Shore A compound reads 91, a nominal 60 reads 78 and a nominal 40 reads 62. That is 11 to 22 points of error, which is larger than the tolerance band on most drawings.

The reading stabilises from about 6 mm. Between 6 and 12 mm the three curves are flat, which is the region the standard is trying to reach. A stack of three 2 mm slabs is acceptable if they are flat and in full contact; a stack of loose pieces with air gaps is not.

The practical consequence is that a part thinner than 6 mm cannot be hardness tested directly. A 2 mm gasket has to be tested as a stack, or the hardness has to be inferred from a plaque moulded from the same compound. Testing the part itself and quoting the number is the most common error in silicone incoming inspection.

Hardness readings falling towards nominal as specimen thickness rises from 1 to 6 millimetres for three grades, and a bar chart of the error introduced by each handling mistake
Left: the same three compounds at different sample thicknesses. Right: what each handling error costs in Shore A points.

Shore A against IRHD

IRHD is the international rubber hardness degree, and it measures the same thing with a different instrument. The IRHD method uses a ball indentor and a different force, and it is designed to be less sensitive to surface condition and more reproducible across laboratories. For most rubbers the two scales agree closely in the middle of the range and diverge at the ends.

Around 50 to 70 Shore A, IRHD and Shore A differ by about one to three points. Below 40 the divergence grows, and above 85 it grows again. A specification that says 60 plus or minus 5 without naming the method is ambiguous, and a supplier and a customer using different methods can disagree on a part that is in fact identical.

IRHD is the better choice for thin sections and for small parts, because the ball indentor is less affected by the support underneath. It is also the more common method in European rubber specifications. Shore A is faster, cheaper and more common in Asia and North America, and for a silicone gasket in the 40 to 70 range the difference rarely matters.

The rule that resolves it is simple: name the method, name the standard, and name the sample thickness in the specification. A drawing that says 60 plus or minus 5 Shore A, ISO 868, on a 6 mm plaque is unambiguous and can be checked. A drawing that says 60 plus or minus 5 hardness cannot.

Sample preparation

The sample has to be flat, parallel and at least 6 mm thick, and it has to be at the test temperature for long enough to be in equilibrium. A sample taken straight from a warm press reads softer than the same sample the next day, because silicone stiffness changes with temperature and because the cure is still completing.

The surface matters too. A moulded surface is smoother than a cut surface, and a cut surface can read one or two points harder because the indentor sits on a rougher plane. For a specification, the sample should be a moulded plaque from the production tool, not a cut piece from a finished part.

The stack, if one is used, must be in full contact with no air gaps and no relative movement. Three pieces of 2 mm sheet stacked loosely will read differently from three pieces bonded together, and neither will match a solid 6 mm slab exactly. The standard accepts a stack but requires the surfaces to be flat and in contact.

Requirement Value Warum
Total thickness At least 6 mm Below that the support affects the reading
Lateral size At least the indentor diameter plus 12 mm Edge effects
Surface Flat, parallel, moulded where possible A rough surface reads harder
Conditioning At 23 C for at least 1 hour Stiffness is temperature dependent
Reading position At least 12 mm from any edge Edge constraint changes the result
Number of readings Five, at least 6 mm apart Silicone is not perfectly uniform

Table 1 — What a valid Shore A sample looks like

Reading the instrument correctly

The instrument has to be held vertically and pressed down until the presser foot is fully in contact with the surface. A reading taken before the foot is seated is high, because the indentor has not yet reached its full penetration. This is the second most common error after sample thickness, and it is worth four to five points.

The reading has to be taken within one second of full contact for most silicone compounds, because the material creeps under the load. A reading taken after five seconds is lower, sometimes by three points, and the standard specifies one second for exactly this reason. Instruments with a maximum hold function help, but the operator still has to read at the right moment.

Temperature matters more than most operators expect. A sample at 5 C reads two points harder than the same sample at 23 C; a sample at 35 C reads two points softer. In an unheated inspection room in winter, this is a real source of disagreement between a supplier in a warm climate and a customer in a cold one.

The instrument itself needs checking. A reference block of known hardness, checked at the start of each session, catches a worn indentor or a tired spring. An instrument that has been in service for years without calibration can be five points out, and nobody notices because the readings are consistent with each other.

Hardness and the properties behind it

Hardness is a proxy for several properties at once, and it is worth knowing which. Higher hardness means higher modulus, higher tensile strength, higher tear strength and lower elongation at break. It also means lower compression set resistance in some compounds, because a harder compound has less ability to relax.

That is why a hardness change is never just a hardness change. A customer who asks for 70 Shore A instead of 60 is also asking for a stiffer part, a stronger part and a part that stretches less. If the application needed the flexibility of 60, the change may solve one problem and create another.

The relationship to compression set is the one that catches people out. A gasket at 70 Shore A seals better against high pressure but conforms less well to a rough surface, and a gasket that does not conform leaks regardless of its hardness. The right hardness is the one that matches the sealing surface, not the highest one available.

For design purposes, a hardness specification should be accompanied by a tolerance on the finished part, not just on the compound. A moulded part can vary by two to three points across a batch because of cure variation, and a specification of plus or minus 3 on the compound plus a process variation of 3 gives a part that can be 6 points away from nominal.

A test method you can defend

The method that survives an audit has four parts: a named standard, a defined sample, a defined number of readings and a defined acceptance rule. Everything else is detail. Without those four, two people can measure the same part and disagree, and neither is wrong.

The acceptance rule should be based on the median of five readings rather than the mean, because a single bad reading from a surface defect can pull a mean out of tolerance. The median is robust to one outlier and is easy to explain to an operator.

Schritt Aktion Record
1 Check the instrument against a reference block Reading against the block value
2 Confirm the sample is at least 6 mm and at 23 C Thickness and temperature
3 Press until the foot is seated, read within 1 s Five readings, 6 mm apart
4 Take the median, not the mean Median and range
5 Compare with the specification and the method Pass or fail against the named standard
6 Keep the sample and the record Traceability to the batch

Table 2 — A Shore A procedure that can be audited

The record is the part that is usually missing. A hardness number without the sample thickness, the temperature and the standard is a number that cannot be defended, and in a dispute about a batch it is worth nothing. A single line on the inspection sheet fixes that permanently.

Why does my 2 mm gasket read 70 Shore A when the drawing says 60?

Because a 2 mm sample is too thin. The indentor feels the support underneath and reads high, typically by 10 to 15 points at that thickness. Test a stack of at least 6 mm, or test a plaque moulded from the same compound.

Is Shore A the same as IRHD?

They measure the same property with different instruments and agree within one to three points between 50 and 70. They diverge below 40 and above 85. A specification should name the method, because a supplier and a customer using different methods can disagree on an identical part.

How long should I wait before reading?

One second after the presser foot is fully seated. Silicone creeps under load, so a reading taken after five seconds is lower by two or three points. The standard specifies one second for that reason.

Can I test hardness on a finished part?

Only if the part is at least 6 mm thick at the measuring point and flat over a diameter larger than the indentor. A curved or thin part cannot be tested directly, and a reading taken on one is not comparable with a plaque reading.

Why do two suppliers give different hardness for the same drawing?

Usually because one is testing a plaque and the other a part, or because one is using Shore A and the other IRHD, or because the conditioning temperature differs. Ask for the method, the sample thickness and the temperature, and the disagreement usually resolves.

Does hardness change with age?

Slightly. Silicone can continue to cure slowly and read one or two points harder after a few weeks, and some compounds soften at high temperature. For critical applications, test after a defined ageing period rather than immediately after moulding.

Hardness readings not matching the drawing?

Send the part, the drawing and the method you are using. We will tell you whether the reading is the material or the measurement.

Ask about hardness testing

Hi there! I'm John, dad and hero to awesome kid. By day, I'm a plastics manufacturing vet — injection molding, extrusion and vacuum forming — who went from factory floors to technical management. Here to share what I've learned—let's grow together!
de_DEDE

Fordern Sie ein schnelles Angebot an

Senden Sie Zeichnungen und detaillierte Anforderungen über

Emial: [email protected]

Oder füllen Sie das untenstehende Kontaktformular aus: