{"id":9332,"date":"2024-01-14T01:00:00","date_gmt":"2024-01-14T01:00:00","guid":{"rendered":"https:\/\/uplastech.com\/silicone-gasket-surface-finish-leak-rate\/"},"modified":"2026-11-08T08:12:03","modified_gmt":"2026-11-08T08:12:03","slug":"silicone-gasket-surface-finish-leak-rate","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ar\/silicone-gasket-surface-finish-leak-rate\/","title":{"rendered":"Silicone Gasket Leak Rate vs Flange Finish: Specifying Ra, Tool Lay and a Helium Test"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n\/* ==UPL-CONVERSION-MODULES-START== 2024 problem-solving \/ lead-gen blocks *\/\n.upl-blog .mod-h{font-size:12.5px;letter-spacing:.12em;text-transform:uppercase;font-weight:700;color:#0d5563;margin:0 0 12px}\n.upl-blog .problem{background:#fff8f3;border:1px solid #f3ddc9;border-left:4px solid #e07a1f;border-radius:10px;padding:22px 26px;margin:0 0 32px;font-size:16px}\n.upl-blog .problem p{margin:0 0 10px}\n.upl-blog .problem p:last-child{margin-bottom:0}\n.upl-blog .problem .mod-h{color:#a85c10}\n.upl-blog .problem .problem-promise{font-weight:700;color:#0b2b33}\n.upl-blog .steps{background:#f7fafb;border:1px solid #e1ebee;border-radius:10px;padding:22px 26px;margin:0 0 28px}\n.upl-blog .steps ol{list-style:none;counter-reset:uplst;margin:0;padding:0}\n.upl-blog .steps li{counter-increment:uplst;position:relative;padding:0 0 16px 42px;margin:0;font-size:15.5px}\n.upl-blog .steps li:last-child{padding-bottom:0}\n.upl-blog .steps li::before{content:counter(uplst);position:absolute;left:0;top:2px;width:26px;height:26px;border-radius:50%;background:#0d5563;color:#fff;font-size:13px;font-weight:700;line-height:26px;text-align:center}\n.upl-blog table.spec th{background:#14707f}\n.upl-blog .conv{background:#eef6f7;border:1px solid #cfe4e8;border-radius:10px;padding:24px 26px;margin:32px 0}\n.upl-blog .conv p{margin:0 0 12px;font-size:15.5px}\n.upl-blog .conv .conv-lbl{font-weight:700;color:#0b2b33;margin:16px 0 8px}\n.upl-blog ul.conv-need{list-style:none;padding:0;margin:0 0 20px;display:grid;grid-template-columns:1fr 1fr;gap:6px 18px}\n.upl-blog ul.conv-need li{position:relative;padding-left:20px;margin:0;font-size:14.5px}\n.upl-blog ul.conv-need li::before{content:\"\";position:absolute;left:0;top:9px;width:9px;height:9px;border:2px solid #14707f;border-radius:2px}\n.upl-blog .conv-btn{display:inline-block;background:#0d5563;color:#fff;text-decoration:none;font-weight:700;padding:11px 22px;border-radius:7px;font-size:15px}\n.upl-blog .checklist{background:#fbfcfd;border:1px solid #e3e9ec;border-radius:10px;padding:24px 26px;margin:36px 0}\n.upl-blog .checklist ul{list-style:none;padding:0;margin:0 0 12px}\n.upl-blog .checklist li{position:relative;padding-left:28px;margin:0 0 10px;font-size:15.5px}\n.upl-blog .checklist li::before{content:\"\";position:absolute;left:0;top:7px;width:14px;height:14px;border:2px solid #0d5563;border-radius:3px}\n.upl-blog .cl-note{font-size:13.5px;color:#6b7280;margin:0}\n.upl-blog .cta .cta-lbl{color:#c9dee3;font-weight:700;margin:0 0 8px;font-size:14.5px}\n.upl-blog ul.cta-need{list-style:none;padding:0;margin:0 0 22px;display:grid;grid-template-columns:1fr 1fr;gap:4px 18px}\n.upl-blog ul.cta-need li{color:#e4f0f2;font-size:14.5px;padding-left:18px;position:relative;margin:0}\n.upl-blog ul.cta-need li::before{content:\"\\2713\";position:absolute;left:0;color:#e07a1f;font-weight:700}\n\/* ==UPL-CONVERSION-MODULES-END== *\/\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}.upl-blog ul.conv-need,.upl-blog ul.cta-need{grid-template-columns:1fr}.upl-blog .problem,.upl-blog .steps,.upl-blog .conv,.upl-blog .checklist{padding:18px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/neoprene-rubber-parts.jpg\" alt=\"Real moulded silicone seals and O-rings made by Uplastech\" width=\"1536\" height=\"909\"><figcaption>Real silicone rubber production context. Uplastech product photo.<\/figcaption><\/figure>\n<div class=\"problem\">\n<p class=\"mod-h\">The problem<\/p>\n<p><b>Symptom.<\/b> A flange assembled with a 2 mm silicone gasket passes a 2 bar air test but is rejected when a helium check at 1 bar returns 5e-5 mbar l\/s against a 1e-6 mbar l\/s limit.<\/p>\n<p><b>What it costs.<\/b> The gasket and bolt load are correct, yet an undefined surface finish on the flange drawing lets each machined batch leak differently, so the delivery and the tooling are disputed.<\/p>\n<p class=\"problem-promise\">This guide links helium leak rate to Ra and tool lay, sets a surface-finish window, and gives a finish clause and acceptance test to put on the gland drawing.<\/p>\n<\/div>\n<div class=\"toc\"><\/div>\n<h2 id=\"why-roughness-not-just-squeeze-sets-the-leak\">Why roughness, not just squeeze, sets the leak<\/h2>\n<p>Helium follows tool marks, so flange roughness, not only squeeze, sets the leak rate. A 2 mm gasket at 20 % squeeze seals a concentric Ra 1.6 um lay, yet a radial Ra 6.3 um scratch leaks 5e-5 mbar l\/s.<\/p>\n<table>\n<thead>\n<tr>\n<th>Helium-test finding<\/th>\n<th>Most likely cause<\/th>\n<th>Confirming check<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Leak worsens as Ra rises<\/td>\n<td>Continuous radial tool marks<\/td>\n<td>Read the lay direction on the trace<\/td>\n<\/tr>\n<tr>\n<td>Mirror-polished face also leaks<\/td>\n<td>Gasket cold-flow and slip<\/td>\n<td>Measure Ra below 0.4 um<\/td>\n<\/tr>\n<tr>\n<td>Leak fixed by more torque<\/td>\n<td>Finish channel, not low load<\/td>\n<td>Re-test after re-machining to Ra 1.6<\/td>\n<\/tr>\n<tr>\n<td>Leak at 2e-7 mbar l\/s<\/td>\n<td>Concentric lay, 20 % squeeze<\/td>\n<td>Accept against the 1e-6 limit<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 - Reading a flange-finish leak-rate dispute<\/p>\n<div class=\"callout\">Record which of these you are actually seeing before changing any setting. Two faults can look identical on the line and need opposite corrections.<\/div>\n<p><!-- upl-conv-v1 quickcta --><\/p>\n<div class=\"quickcta\">\n<p class=\"mod-h\">Need a fixed price for this seal?<\/p>\n<p>Send the gland drawing, temperature range, media and annual volume. We will recommend a compound with test data and return samples with a written production quotation.<\/p>\n<p class=\"quickcta-act\"><a class=\"quickcta-btn\" href=\"https:\/\/uplastech.com\/silicone-rubber\/\">Get a silicone seal quotation<\/a><a class=\"quickcta-alt\" href=\"mailto:john@uplastech.com\">Email john@uplastech.com<\/a><a class=\"quickcta-alt\" href=\"https:\/\/wa.me\/8617717529949\">WhatsApp<\/a><\/p>\n<\/div>\n<h2 id=\"measure-ra-and-the-tool-lay\">Measure Ra and the tool lay<\/h2>\n<p>Measure the flange with a stylus profilometer at four points, logging Ra and lay, then helium-test at 1 bar for 10 s. The chart below plots leak rate against Ra for two tool lays against a 1e-6 mbar l\/s limit.<\/p>\n<div class=\"steps\">\n<p class=\"mod-h\">A five-step diagnostic sequence<\/p>\n<ol>\n<li><b>Log the drawing and the finish note.<\/b><br \/>Confirm whether Ra and lay were ever written on the gland drawing or only quoted in an email.<\/li>\n<li><b>Measure Ra and lay at four points.<\/b><br \/>Use a stylus profilometer; record Ra 0.8-1.6 um and the tool direction relative to the seal.<\/li>\n<li><b>Helium-test the assembled joint.<\/b><br \/>Hold 1 bar helium for 10 s on five flanges and record leak rate in mbar l\/s.<\/li>\n<li><b>Re-machine one flange to the clause.<\/b><br \/>Bring it to Ra 1.6 um concentric lay, then re-test to show the leak drops below 1e-6 mbar l\/s.<\/li>\n<li><b>Agree the acceptance record.<\/b><br \/>Put Ra 0.8-1.6 um, concentric lay and the 1e-6 mbar l\/s limit on the purchase order.<\/li>\n<\/ol>\n<\/div>\n<p>The chart below is a typical result from that measurement step. Use it to separate a design limit from a setting that can still be recovered.<\/p>\n<figure>\n<img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/silicone-gasket-surface-finish-leak-rate-chart.jpg\" alt=\"Silicone Gasket Leak Rate vs Flange Finish: Specifying Ra, Tool Lay and a Helium Test: calculated response trend and an illustrative root-cause split\" width=\"1536\" height=\"909\"><figcaption>Figure 1 \u2014 Calculated response trend and an illustrative root-cause split. Values are engineering guidance for diagnosis, not a measured survey; confirm them on your own line before changing a drawing or a specification.<\/figcaption><\/figure>\n<h2 id=\"specify-the-surface-finish-window\">Specify the surface-finish window<\/h2>\n<p>Specify Ra 0.8-1.6 um with a concentric lay, 20 % squeeze on a 2 mm gasket, and a helium leak below 1e-6 mbar l\/s. Above Ra 3.2 um radial channels open; below 0.4 um a polished face lets the gasket slip.<\/p>\n<table class=\"spec\">\n<thead>\n<tr>\n<th>Parameter<\/th>\n<th>Typical target<\/th>\n<th>What goes wrong outside it<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Flange roughness Ra<\/td>\n<td>0.8 - 1.6 um<\/td>\n<td>Above 3.2 um radial channels leak<\/td>\n<\/tr>\n<tr>\n<td>Tool lay<\/td>\n<td>Concentric to the seal<\/td>\n<td>Radial marks give helium a path<\/td>\n<\/tr>\n<tr>\n<td>Gasket squeeze<\/td>\n<td>20 % on a 2 mm section<\/td>\n<td>Below 15 % the gasket cannot fill valleys<\/td>\n<\/tr>\n<tr>\n<td>Helium leak rate<\/td>\n<td>Below 1e-6 mbar l\/s at 1 bar<\/td>\n<td>A radial scratch reaches 5e-5 mbar l\/s<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 - Surface-finish and leak parameters for the gland drawing<\/p>\n<h2 id=\"put-the-finish-clause-on-the-gland-drawing\">Put the finish clause on the gland drawing<\/h2>\n<p>Write the surface finish on the gland drawing, not in an email: Ra 0.8-1.6 um, lay concentric to the seal, no radial scratches, and a 1e-6 mbar l\/s helium limit at 1 bar. Require a profilometer trace and a leak certificate per batch.<\/p>\n<table>\n<thead>\n<tr>\n<th>Option<\/th>\n<th>When it fits<\/th>\n<th>Trade-off<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Re-machine to Ra 0.8-1.6 um concentric<\/td>\n<td>Radial or coarse finish<\/td>\n<td>Machining time and scrap<\/td>\n<\/tr>\n<tr>\n<td>Add a PTFE envelope gasket<\/td>\n<td>Finish cannot be changed<\/td>\n<td>Extra part and cost<\/td>\n<\/tr>\n<tr>\n<td>Raise squeeze above 20 %<\/td>\n<td>Rarely sufficient<\/td>\n<td>Over-compression, faster creep<\/td>\n<\/tr>\n<tr>\n<td>Write a 1e-6 mbar l\/s clause<\/td>\n<td>Future orders<\/td>\n<td>Narrower machining options<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 - Corrective paths for a rough-flange leak<\/p>\n<div class=\"myth\"><b>Myth:<\/b> \"A process adjustment will fix it.\" Once a design limit is reached, more tuning only adds cost and variation. Confirm the limit with a measurement, then change the drawing or the specification.<\/div>\n<h2 id=\"confirm-with-a-helium-leak-test\">Confirm with a helium leak test<\/h2>\n<p>Confirm the clause with a helium mass-spectrometer test at 1 bar for 10 s on five flanges machined to Ra 1.6 um concentric lay. A joint reading 2e-7 mbar l\/s passes with margin; re-machine any flange whose radial trace breaches the 1e-6 limit.<\/p>\n<div class=\"conv\">\n<p class=\"mod-h\">Want a compound check before you re-order?<\/p>\n<p>Send us the gland drawing and the service conditions. We will compare the compound data against your temperature range and return a recommendation with sample parts.<\/p>\n<p class=\"conv-lbl\">What to send us<\/p>\n<ul class=\"conv-need\">\n<li>Gland dimensions and cross-section<\/li>\n<li>Temperature range and media<\/li>\n<li>A failed seal if available<\/li>\n<li>Annual volume<\/li>\n<\/ul>\n<p><a class=\"conv-btn\" href=\"\/silicone-rubber\/\">Send the gland drawing<\/a>\n<\/div>\n<h2 id=\"close-the-claim-with-a-profilometer-trace\">Close the claim with a profilometer trace<\/h2>\n<p>Recover the held lot by re-measuring Ra and lay on four points per flange and re-testing at 1 bar helium. If the finish is outside 0.8-1.6 um, re-machine rather than adding torque; tightening the joint only hides a continuous scratch.<\/p>\n<div class=\"callout\">Validate one change at a time and keep the measurement record. A supplier discussion backed by data is resolved in days, not weeks.<\/div>\n<div class=\"checklist\">\n<p class=\"mod-h\">Before you release this silicone seal<\/p>\n<ul>\n<li>Ra 0.8-1.6 um and a concentric tool lay are dimensioned on the gland drawing<\/li>\n<li>Radial scratches across the sealing face are explicitly prohibited<\/li>\n<li>A 20 % squeeze on the 2 mm gasket is stated with the groove depth<\/li>\n<li>A helium test at 1 bar for 10 s with a 1e-6 mbar l\/s limit is in the purchase order<\/li>\n<li>A profilometer trace and a leak certificate are required per production batch<\/li>\n<\/ul>\n<p class=\"cl-note\">Most cold or heat failures are specification gaps, not bad batches. Fix the specification before changing suppliers.<\/p>\n<\/div>\n<div class=\"faq\">\n<h3>Why does a rougher flange leak more?<\/h3>\n<p>Radial tool marks form a continuous channel from the bore to the outer edge. A Ra 6.3 um radial scratch can pass 5e-5 mbar l\/s even at 20 % squeeze.<\/p>\n<h3>Can a very smooth flange be as bad?<\/h3>\n<p>Yes. Below about Ra 0.4 um the polished face gives no grip, so the gasket cold-flows and slips, opening a leak. Target 0.8-1.6 um.<\/p>\n<h3>What squeeze should we specify?<\/h3>\n<p>20 % on a 2 mm gasket, compressing it to 1.60 mm. Too little squeeze leaves valleys unfilled; too much accelerates creep and relaxation.<\/p>\n<h3>What leak limit is realistic?<\/h3>\n<p>Below 1e-6 mbar l\/s at 1 bar helium. A concentric Ra 1.6 um lay typically reaches 2e-7 mbar l\/s, comfortably inside the clause.<\/p>\n<h3>Will more bolt torque fix a rough flange?<\/h3>\n<p>No. Extra load hides a continuous scratch without sealing it. Re-machine to Ra 0.8-1.6 um concentric lay and re-test.<\/p>\n<h3>How do we prevent a repeat dispute?<\/h3>\n<p>Write Ra, lay direction, squeeze and the helium limit on the gland drawing, and require a profilometer trace and leak certificate per batch.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Get a seal specified for the real service conditions<\/p>\n<p>Send us the gland drawing and the service conditions. We will recommend a compound with documented test data, review the squeeze, and supply samples with a production quotation.<\/p>\n<p class=\"cta-lbl\">To get an accurate quote, send:<\/p>\n<ul class=\"cta-need\">\n<li>Gland drawing or seal cross-section<\/li>\n<li>Temperature range and media<\/li>\n<li>Pressure and movement<\/li>\n<li>Annual volume and target unit price<\/li>\n<\/ul>\n<p><a class=\"btn\" href=\"\/silicone-rubber\/\">Request samples and a quotation<\/a><br \/>\n<!-- upl-conv-v1 contact --><\/p>\n<div class=\"contactbar\">\n<p class=\"contactbar-h\">Prefer to talk it through first?<\/p>\n<p>Email <a href=\"mailto:john@uplastech.com\">john@uplastech.com<\/a> or message us on <a href=\"https:\/\/wa.me\/8617717529949\">WhatsApp +86 177 1752 9949<\/a>. Send a drawing, a sample or a specification and an engineer will reply.<\/p>\n<\/div>\n<p><!-- upl-conv-v1 trust --><\/p>\n<div class=\"trust\">\n<p class=\"trust-h\">Why buyers work with Uplastech<\/p>\n<p>ISO 9001, ISO 14001 and ISO 45001 certified. Founded in 2016, with injection moulding lines in Shanghai and an extrusion plant in Jiangsu. Moulding machines from 90T to 1100T and a maximum shot weight of 5100 g. Samples and a written quotation are available on request.<\/p>\n<\/div>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/silicone-compression-set\/\">Silicone compression set<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/silicone-gasket-seal\/\">Silicone gasket and seal design<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/silicone-hardness-shore-a\/\">Silicone hardness: Shore A<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/silicone-industrial-seals\/\">Silicone industrial seals<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/silicone-o-ring-manufacturing\/\">Silicone o-ring manufacturing<\/a><\/li>\n<\/ul>\n<p><!-- upl-conv-v1 service --><\/p>\n<p class=\"rel-svc\">Ready to specify? See our <a href=\"https:\/\/uplastech.com\/silicone-rubber\/\">silicone rubber moulding services<\/a> or <a href=\"mailto:john@uplastech.com\">request a written quotation<\/a>.<\/p>\n<\/div>\n<\/div>\n<p><script type=\"application\/ld+json\">{\"@context\": \"https:\/\/schema.org\", \"@type\": \"FAQPage\", \"mainEntity\": [{\"@type\": \"Question\", \"name\": \"Why does a rougher flange leak more?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"Radial tool marks form a continuous channel from the bore to the outer edge. A Ra 6.3 um radial scratch can pass 5e-5 mbar l\/s even at 20 % squeeze.\"}}, {\"@type\": \"Question\", \"name\": \"Can a very smooth flange be as bad?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"Yes. Below about Ra 0.4 um the polished face gives no grip, so the gasket cold-flows and slips, opening a leak. Target 0.8-1.6 um.\"}}, {\"@type\": \"Question\", \"name\": \"What squeeze should we specify?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"20 % on a 2 mm gasket, compressing it to 1.60 mm. Too little squeeze leaves valleys unfilled; too much accelerates creep and relaxation.\"}}, {\"@type\": \"Question\", \"name\": \"What leak limit is realistic?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"Below 1e-6 mbar l\/s at 1 bar helium. A concentric Ra 1.6 um lay typically reaches 2e-7 mbar l\/s, comfortably inside the clause.\"}}, {\"@type\": \"Question\", \"name\": \"Will more bolt torque fix a rough flange?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"No. Extra load hides a continuous scratch without sealing it. Re-machine to Ra 0.8-1.6 um concentric lay and re-test.\"}}, {\"@type\": \"Question\", \"name\": \"How do we prevent a repeat dispute?\", \"acceptedAnswer\": {\"@type\": \"Answer\", \"text\": \"Write Ra, lay direction, squeeze and the helium limit on the gland drawing, and require a profilometer trace and leak certificate per batch.\"}}]}<\/script><\/p>\n","protected":false},"excerpt":{"rendered":"<p>This guide links helium leak rate to Ra and tool lay, sets a surface-finish window, and gives a finish clause and acceptance test to put on the gland drawing.<\/p>","protected":false},"author":1,"featured_media":7393,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[39],"tags":[],"class_list":["post-9332","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-silicone-rubber-products"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/9332","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/comments?post=9332"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/9332\/revisions"}],"predecessor-version":[{"id":9917,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/9332\/revisions\/9917"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media\/7393"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media?parent=9332"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/categories?post=9332"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/tags?post=9332"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}