{"id":8731,"date":"2026-08-16T09:00:00","date_gmt":"2026-08-16T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/extrusion-die-lines\/"},"modified":"2026-11-02T02:25:35","modified_gmt":"2026-11-02T02:25:35","slug":"extrusion-die-lines","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ar\/extrusion-die-lines\/","title":{"rendered":"Die Lines: Tracing a Longitudinal Mark Back to Its Source"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/extrusion-die-lines.jpg\" alt=\"A white PVC window profile held up by a gloved hand with a single faint longitudinal line running along its glossy face\" width=\"1536\" height=\"909\"><figcaption>One line, continuous for the whole coil, and it starts at the die.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"what\">A die line is a scratch, copied<\/h2>\n<p>A die line is a longitudinal mark on an extruded profile that runs parallel to the extrusion direction and continues without interruption for as long as the line runs. That continuity is the diagnostic: anything that appears and disappears, or that wanders across the face, is not a die line, it is a downstream mark or a melt defect.<\/p>\n<p>The mechanism is a copy. The polymer slides along the die land, the final parallel section of the flow channel, at a shear rate that can exceed 100 per second. Any irregularity on that land, a scratch, a pit, a burr, a patch of degraded material stuck to the wall, disturbs the flow locally and leaves a corresponding ridge or groove in the surface of the extrudate. The mark then passes through the calibration sleeve, the water bath and the haul-off unchanged, because nothing downstream smooths it.<\/p>\n<p>This is why die lines are so persistent. A scratch of a few micrometres on a hardened steel land produces a visible line on a glossy surface, and the line is regenerated continuously. Polishing it out once fixes it permanently, provided the cause of the scratch is also removed, which is usually a piece of grit, a burr on the die lip, or a cleaning tool used too enthusiastically.<\/p>\n<p>The distinction that matters most is between a die line and a melt fracture line. Both are longitudinal. A die line is sharp, has a defined position that does not move with output rate, and is visible even at low speed. A melt fracture line is a roughness or a helical pattern that appears above a critical shear rate and disappears when the output is reduced. One is a surface problem, the other is a flow problem, and they have different fixes.<\/p>\n<h2 id=\"depth\">The mark depth follows the land roughness<\/h2>\n<p>The chart on the left plots mark depth against die land roughness for a typical rigid PVC profile. At Ra 0.2 micrometres the mark is about 2 micrometres deep, at 0.4 it is 5, at 0.8 it is 12, at 1.6 it is 26 and at 3.2 it is 48. The visible limit on a glossy white surface is around 10 micrometres, which the dashed line marks.<\/p>\n<figure>\n<img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/extrusion-die-lines-chart.jpg\" alt=\"Mark depth against die land roughness with a visible limit line, and a bar chart of die line causes\" width=\"1536\" height=\"909\"><figcaption>Left: polishing below Ra 0.8 takes the mark under the visible limit. Right: half of all cases start on the land surface.<\/figcaption><\/figure>\n<p>The relationship is steeper than linear because the mark is not simply a scaled copy of the scratch. A rougher land disturbs the flow over a larger region and the elastic recovery of the polymer after the die amplifies the disturbance. Doubling the roughness roughly triples the mark depth in the visible range.<\/p>\n<p>The practical target is Ra 0.4 to 0.8 micrometres on any land that produces a visible face. That is a polished finish, achieved with a sequence of abrasives down to 800 or 1000 grit followed by a felt wheel and a polishing compound. It is a two hour job for a competent toolmaker and it is the difference between a profile that sells and one that is discounted.<\/p>\n<p>The right hand panel shows where die lines actually come from: die land damage 30 percent, carbon build-up 24, poor polishing 18, melt fracture 14, a foreign particle 8. Land damage and carbon together are 54 percent, and both are surface conditions rather than design faults. Poor polishing at 18 percent is the original sin, the die that was never finished properly and has produced marginal profiles since day one.<\/p>\n<h2 id=\"carbon\">Carbon build-up is a slow die line<\/h2>\n<p>Carbon build-up, sometimes called die drool or plate-out depending on the material, is degraded polymer that has stuck to the die wall and partially charred. It starts as a thin film, grows into a ridge, and eventually a fragment breaks off and leaves a comet-shaped defect that is much worse than the line it preceded.<\/p>\n<p>The cause is a combination of residence time, temperature and formulation. Polymer that sits in a low-flow region near the die lip, or in a dead spot behind an insert, degrades slowly. PVC is particularly prone because it degrades by dehydrochlorination, which is autocatalytic: once it starts, it accelerates. A die that runs continuously for weeks without cleaning will build up carbon regardless of how good the formulation is.<\/p>\n<p>The control measures are practical rather than theoretical. Purge the die on a schedule rather than when the line looks bad. Keep the die lip temperature above the melt temperature so the polymer at the wall does not freeze. Avoid dead spots in the flow channel when the die is designed. And check the stabiliser package, because a formulation that is marginal on thermal stability will build carbon faster than one that is not.<\/p>\n<h2 id=\"diagnose\">Diagnosing which one you have<\/h2>\n<p>The first test is to change the output rate. If the mark stays at the same position and the same depth at half speed, it is a die line. If it fades or disappears, it is melt fracture or a related flow instability, and the answer is a higher melt temperature, a lower shear rate, or a different land length.<\/p>\n<p>The second test is to change the material. If a different compound on the same die produces the same line in the same place, the die is the cause. If the line moves or changes, the material is implicated, usually through its lubricant balance or its filler content.<\/p>\n<p>The third test is visual and it is decisive. Stop the line, clean the die face, and inspect the land under a bright light with a magnifier. A scratch, a pit or a carbon ridge will be visible. Most die lines are found this way in ten minutes, and the argument about formulation ends there.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0627\u0644\u0645\u064a\u0632\u0629<\/th>\n<th>Die line<\/th>\n<th>Melt fracture line<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Position<\/td>\n<td>Fixed, does not move with rate<\/td>\n<td>Moves or changes with rate<\/td>\n<\/tr>\n<tr>\n<td>Depth against output<\/td>\n<td>Constant<\/td>\n<td>Rises sharply above a critical rate<\/td>\n<\/tr>\n<tr>\n<td>\u0627\u0644\u0645\u0638\u0647\u0631<\/td>\n<td>Sharp, defined<\/td>\n<td>Rough, often helical<\/td>\n<\/tr>\n<tr>\n<td>\u0627\u0644\u0633\u0628\u0628<\/td>\n<td>Land damage, carbon, polishing<\/td>\n<td>Shear rate above the material limit<\/td>\n<\/tr>\n<tr>\n<td>Fix<\/td>\n<td>Polish or clean the land<\/td>\n<td>Raise temperature, reduce rate, change land length<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 Telling a die line from a melt fracture line.<\/p>\n<h2 id=\"polish\">Polishing a land back<\/h2>\n<p>The repair is a sequence, and skipping a step makes it worse. Start with the finest abrasive that will remove the defect, not the coarsest available. A 400 grit stone on a 0.5 micrometre scratch creates a 400 grit scratch, which is deeper than what you were trying to remove.<\/p>\n<p>Work along the flow direction, never across it. A scratch across the land produces a mark that is continuous around the profile rather than along it, which is a far more visible defect. Keep the abrasive flat and use a backing block on a flat land so the surface stays planar; a rounded land changes the flow and the die no longer produces the intended dimensions.<\/p>\n<p>Finish with a felt wheel and a diamond or aluminium oxide compound, then clean the die thoroughly. Polishing compound left in a corner of the flow channel becomes a source of contamination and, in PVC, of degradation. A die that is polished and not cleaned produces a line from the residue within a shift.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0627\u0644\u062e\u0637\u0648\u0629<\/th>\n<th>Abrasive<\/th>\n<th>\u0627\u0644\u063a\u0631\u0636<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Defect removal<\/td>\n<td>600 to 800 grit stone<\/td>\n<td>Remove the scratch without deepening it<\/td>\n<\/tr>\n<tr>\n<td>\u0627\u0644\u0645\u0632\u062c<\/td>\n<td>1000 to 1200 grit paper<\/td>\n<td>Flatten the scratch pattern<\/td>\n<\/tr>\n<tr>\n<td>Polish<\/td>\n<td>Felt wheel with compound<\/td>\n<td>Bring Ra to 0.4 to 0.8 micrometres<\/td>\n<\/tr>\n<tr>\n<td>Clean<\/td>\n<td>Solvent and lint-free cloth<\/td>\n<td>Remove all compound residue<\/td>\n<\/tr>\n<tr>\n<td>\u062a\u062d\u0642\u0642<\/td>\n<td>Magnifier and a short run<\/td>\n<td>Confirm the line has gone<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 The polishing sequence for a die land.<\/p>\n<h2 id=\"prevent\">Preventing the next one<\/h2>\n<p>The most common cause of a repeat scratch is the cleaning method. A brass scraper, a screwdriver or a wire brush used to remove carbon from a die face will scratch a polished land every time. The correct tools are soft, and the correct method is a soak in a proper cleaning salt or solvent followed by a soft brush.<\/p>\n<p>The second is handling. A die that is removed and set down on a bench face-first will pick up a scratch from the bench. Dies should be stored face-up on a soft surface, with the land protected by a cover, and moved with a lifting frame rather than by hand.<\/p>\n<p>The third is the screw and barrel. A worn screw delivers unmelted particles that damage the land as they pass, and a barrel with a groove or a dead spot delivers degraded material that sticks to it. If die lines recur on a die that is polished and clean, look upstream at the screw and the barrel before polishing again.<\/p>\n<div class=\"faq\">\n<h3>What causes a die line on an extruded profile?<\/h3>\n<p>A defect on the die land, the final parallel section of the flow channel. A scratch, a pit, a burr or a patch of carbon disturbs the flow and leaves a continuous mark on the extrudate. Because the land is where the surface is formed, the mark is regenerated on every metre.<\/p>\n<h3>How do I tell a die line from a melt fracture line?<\/h3>\n<p>Change the output rate. A die line stays at the same position and depth at half speed; a melt fracture line fades or disappears. A die line is also sharper and more defined, while melt fracture looks rough and often helical.<\/p>\n<h3>What die land roughness should I aim for?<\/h3>\n<p>Ra 0.4 to 0.8 micrometres on any face that will be visible. At Ra 0.8 the mark is around 12 micrometres deep, just above the visible limit; at 0.4 it is about 5 and invisible. Polishing below 0.4 rarely gains anything.<\/p>\n<h3>Can a die line be polished out?<\/h3>\n<p>Yes, if it is caused by the land surface. Use the finest abrasive that removes the defect, work along the flow direction, finish with a felt wheel to Ra 0.4 to 0.8, and clean thoroughly. Then find and remove the cause, or the line will return.<\/p>\n<h3>Why do die lines come back after polishing?<\/h3>\n<p>Because the cause was not removed. Recurring lines usually mean a worn screw delivering unmelted particles, a barrel dead spot feeding degraded material, or a cleaning method that scratches the land. Look upstream before polishing a third time.<\/p>\n<h3>Does the material affect die lines?<\/h3>\n<p>Yes, indirectly. A formulation with a poor lubricant balance or marginal thermal stability builds carbon on the land faster, and carbon is the second largest cause. A rigid PVC with an inadequate stabiliser will produce lines from degradation rather than from damage.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Chasing a line on a profile<\/p>\n<p>Send a photo of the mark and tell us where it sits on the section. We can usually tell from the position whether it is a land defect, a flow problem or a downstream mark, and what to check first.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ar\/%d9%85%d9%84%d8%a7%d9%85%d8%ad-%d8%a8%d9%88%d9%84%d9%8a-%d9%83%d9%84%d9%88%d8%b1%d9%8a%d8%af-%d8%a7%d9%84%d9%81%d9%8a%d9%86%d9%8a%d9%84-%d9%85%d8%aa%d8%b9%d8%af%d8%af-%d8%a7%d9%84%d9%81%d9%8a%d9%86\/\">Discuss a profile defect<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ar\/extrusion-die-flow-channel\/\">Extrusion Die Flow Channel Design<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/extrusion-die-swell\/\">Die Swell and What It Does to Dimensions<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/extruder-screw-wear\/\">Extruder Screw Wear: Symptoms and Effects<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/extrusion-profile-tolerance\/\">Extrusion Profile Tolerance: What Can Be Held<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/sheet-surface-gloss\/\">Sheet Surface Gloss: Causes and Control<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>A die line is a scratch on the die land copied onto every metre of profile. The mark depth tracks the land roughness almost exactly, which is why the answer is usually polishing rather than a new die.<\/p>","protected":false},"author":1,"featured_media":8729,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[17],"tags":[],"class_list":["post-8731","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-plastic-extrusion-process"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/8731","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/comments?post=8731"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/8731\/revisions"}],"predecessor-version":[{"id":8820,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/8731\/revisions\/8820"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media\/8729"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media?parent=8731"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/categories?post=8731"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/tags?post=8731"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}