{"id":8052,"date":"2026-01-23T09:00:00","date_gmt":"2026-01-23T09:00:00","guid":{"rendered":"https:\/\/uplastech.com\/back-pressure-screw-recovery\/"},"modified":"2026-01-23T09:00:00","modified_gmt":"2026-01-23T09:00:00","slug":"back-pressure-screw-recovery","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ar\/back-pressure-screw-recovery\/","title":{"rendered":"Back Pressure: Consistency Is Bought in Heat"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae\u3002\n   \u6ce8\u610f\uff1aClick to Chat \u7684\u70b9\u51fb\u903b\u8f91\u662f\u300c\u95ee\u5019\u5361\u5143\u7d20\u5b58\u5728\u5c31\u4e0d\u8df3\u8f6c\u300d\uff0c\u53ea\u9760 CSS \u9690\u85cf\u4f1a\u8ba9\u6c14\u6ce1\u53d8\u6210\u6b7b\u94fe\u63a5\u3002\n   Code Snippets #9\u300cUPL single post: WhatsApp bubble jumps straight to chat\u300d\u8d1f\u8d23\u628a\u8be5\u8282\u70b9\u4ece DOM \u79fb\u9664\uff0c\n   \u4e0b\u9762\u8fd9\u6761 CSS \u53ea\u662f\u79fb\u9664\u524d\u7684\u89c6\u89c9\u515c\u5e95\u3002\u5220 #9 \u524d\u5fc5\u987b\u5148\u5220\u8fd9\u6761\u89c4\u5219\u3002 *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/back-pressure-screw-recovery.jpg\" alt=\"Injection moulding machine with the screw withdrawn from the barrel, a technician in a blue jacket reading the control screen\" width=\"1536\" height=\"909\"><figcaption>A screw out of its barrel. Back pressure is the resistance it works against while it turns, and that resistance is what makes the shot repeatable.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"what\">Back pressure is resistance during recovery, not during injection<\/h2>\n<p>Back pressure is applied while the screw is rotating and retracting, not while it is injecting. It is a hydraulic resistance on the screw that the melt must overcome to push the screw back, and its job is to compact the melt, squeeze out air and mix the material as it passes through the check ring.<\/p>\n<p>The confusion is common because the number appears on the same screen as the injection pressure. Injection pressure drives the screw forward and fills the cavity. Back pressure resists the screw moving back and prepares the next shot. They act on the same screw at different times and they do opposite things.<\/p>\n<p>With no back pressure the screw retracts as fast as the melt arrives, the check ring does not seat properly, and the shot volume is whatever happened to be in front of the screw. That is why zero back pressure produces the worst shot-to-shot variation on any machine.<\/p>\n<h2 id=\"curve\">Consistency has a floor and it is reached early<\/h2>\n<p>Shot weight variation against back pressure: 0.90 percent at zero, 0.50 at 5 bar, 0.30 at 10, 0.25 at 20 and 0.24 at 30. The first 10 bar removes two thirds of the variation. The next 20 bar removes 0.06 percentage points.<\/p>\n<p>The mechanism behind the flattening is that the melt is already compact. Once the check ring has seated and the air has been squeezed out, more resistance does not make the melt more compact, it just shears it harder against the barrel wall. The shear generates heat, and the heat is what the rest of the curve costs.<\/p>\n<p>That makes 10 to 15 bar the useful range for most materials. Above it the machine is working harder, the melt is hotter, and the shot weight is no more repeatable than it was at 10 bar.<\/p>\n<h2 id=\"heat\">The heat is not a side effect, it is the bill<\/h2>\n<p>Melt temperature rise against back pressure: 0 degrees at zero, 3 at 5 bar, 7 at 10, 16 at 20 and 26 at 30. The rise is not linear, because shear heating depends on the shear rate and on the viscosity at that shear rate, and both change as the pressure rises.<\/p>\n<p>A 26 degree rise is enough to change the material. It shortens the cooling time needed, which sounds good, and it moves the melt further along its degradation curve, which does not. For a heat-sensitive material like PVC or a flame-retardant compound, 26 degrees is the difference between a stable process and one that produces black specks after an hour.<\/p>\n<p>It also makes the process harder to control, because the shear heating depends on the screw speed and on the melt viscosity, which depends on the temperature. A high back pressure combined with a high screw speed is a feedback loop: more heat, lower viscosity, more flow, more shear, more heat.<\/p>\n<figure>\n<img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/back-pressure-screw-recovery-chart.jpg\" alt=\"Shot weight variation against back pressure, and melt temperature rise against the same pressure\" width=\"1536\" height=\"909\"><figcaption>Shot weight variation falls from 0.90 to 0.30 percent over the first 10 bar, while melt temperature rises 26 degrees across the full range.<\/figcaption><\/figure>\n<h2 id=\"recovery\">Screw recovery is the other half of the setting<\/h2>\n<p>Back pressure is one of three settings that control recovery. The other two are screw speed and the decompression, or suck-back, after recovery finishes. All three affect the shot, and they are usually set by whoever was on the machine first.<\/p>\n<table>\n<thead>\n<tr>\n<th>Setting<\/th>\n<th>What it controls<\/th>\n<th>Wrong value does what<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Back pressure<\/td>\n<td>Melt compaction and mixing<\/td>\n<td>Too low: shot varies. Too high: degraded melt<\/td>\n<\/tr>\n<tr>\n<td>\u0633\u0631\u0639\u0629 \u0627\u0644\u0644\u0648\u0644\u0628<\/td>\n<td>Recovery time and shear rate<\/td>\n<td>Too high: shear heat and unmelted pellets carried forward<\/td>\n<\/tr>\n<tr>\n<td>Decompression<\/td>\n<td>Pressure release before injection<\/td>\n<td>Too much: drool and air. Too little: nozzle freeze<\/td>\n<\/tr>\n<tr>\n<td>Cushion<\/td>\n<td>Material left after the shot<\/td>\n<td>Too small: no packing. Too large: long residence time<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 The four settings that decide whether the next shot is the same as the last<\/p>\n<p>The cushion is the one that gets ignored and matters most. A cushion of 3 to 6 mm means the machine had material left to pack with. A cushion near zero means the shot used everything available and the part was never packed, which shows up as sink and as short shots at the end of a run rather than at the start.<\/p>\n<h2 id=\"set\">Setting it from the material, not from the last job<\/h2>\n<p>Back pressure is usually quoted as a hydraulic pressure, which is machine-specific. Two machines with different screw diameters will produce different melt pressures at the same hydraulic setting, so a value copied from another machine is meaningless. Set it as a percentage of the machine's maximum, then verify by the effect rather than by the number.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0627\u0644\u0645\u0648\u0627\u062f<\/th>\n<th>Typical back pressure<\/th>\n<th>Reason<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Polypropylene, polyethylene<\/td>\n<td>5 to 12 bar<\/td>\n<td>Tolerant, low shear sensitivity<\/td>\n<\/tr>\n<tr>\n<td>ABS, polystyrene<\/td>\n<td>8 to 15 bar<\/td>\n<td>Needs mixing, moderate sensitivity<\/td>\n<\/tr>\n<tr>\n<td>\u0628\u0648\u0644\u064a \u0643\u0631\u0628\u0648\u0646\u0627\u062a<\/td>\n<td>10 to 20 bar<\/td>\n<td>High viscosity, needs compaction<\/td>\n<\/tr>\n<tr>\n<td>PVC, rigid<\/td>\n<td>3 to 8 bar<\/td>\n<td>Very heat sensitive, keep the shear low<\/td>\n<\/tr>\n<tr>\n<td>Glass-filled grades<\/td>\n<td>8 to 15 bar<\/td>\n<td>Mixing matters, but fibre damage rises with shear<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 Starting points by material, to be verified on the machine<\/p>\n<p>Then verify with a shot weight study: twenty shots at each setting, weighed, and the standard deviation calculated. The curve will flatten at a different pressure on every machine, and the flattening point is the setting, not the number in the table.<\/p>\n<h2 id=\"specify\">What to specify<\/h2>\n<p>A recovery specification has to describe the outcome as well as the settings.<\/p>\n<ul>\n<li>Back pressure as a percentage of machine maximum, not as an absolute hydraulic value.<\/li>\n<li>Screw speed, in rpm, with the recovery time it produces.<\/li>\n<li>Cushion, in mm, with the minimum acceptable value.<\/li>\n<li>Decompression, in mm, and whether the nozzle is shut off mechanically.<\/li>\n<li>Shot weight variation, as a standard deviation over twenty shots, which is the number the settings exist to control.<\/li>\n<\/ul>\n<p>The shot weight number is the one to hold the process to. Settings drift between machines and between shifts, but a standard deviation under 0.3 percent means the process is doing what it was set up to do, whatever the numbers on the screen say.<\/p>\n<div class=\"myth\">Myth: more back pressure means better mixing and a better part. Past about 15 bar on most materials the shot weight stops improving and the melt temperature keeps climbing, and the extra heat costs colour, cooling time and degradation. The right setting is where the curve flattens, not where the operator feels confident.<\/div>\n<div class=\"faq\">\n<h3>What does back pressure actually do?<\/h3>\n<p>It resists the screw as it retracts during recovery, which compacts the melt, squeezes out air and forces the material through the check ring so it mixes.<\/p>\n<h3>How much back pressure should I use?<\/h3>\n<p>10 to 15 bar on most materials, set as a percentage of machine maximum. Above that the shot weight stops improving.<\/p>\n<h3>Why does back pressure raise the melt temperature?<\/h3>\n<p>Shear heating. The melt is forced through a narrow gap at the check ring, and the energy goes into the material rather than into moving the screw.<\/p>\n<h3>What is cushion and why does it matter?<\/h3>\n<p>The material left in front of the screw after injection, usually 3 to 6 mm. It is what the packing phase uses; without it the part is never packed.<\/p>\n<h3>Can I copy back pressure between machines?<\/h3>\n<p>No. Hydraulic pressure produces a different melt pressure on a machine with a different screw diameter. Copy the percentage and verify by shot weight.<\/p>\n<h3>How do I know the setting is right?<\/h3>\n<p>Weigh twenty shots and calculate the standard deviation. The right setting is where that number stops falling as pressure rises.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">A shot weight that will not settle?<\/p>\n<p>Send the material, the shot weight and the current recovery settings. We will tell you where the consistency curve flattens on your machine and what the heat costs.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ar\/custom-injection-molding\/\">Ask about process setting<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ar\/injection-speed-profiling\/\">Injection Speed Profiling: The Fastest Fill Is Not the Cheapest<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/melt-temperature-barrel-profile\/\">Barrel Temperature Profile: Flat, Rising or Falling<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/cooling-time-optimization\/\">Cooling Time: Three Times the Wall Is Nine Times the Wait<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/clamp-force-tonnage\/\">Clamp Force: You Cannot Size a Tonnage From a Table<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/custom-injection-molding\/\">Custom Injection Moulding: Tooling, Materials and Tolerances<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Shot weight variation falls from 0.90 percent to 0.30 as back pressure goes from zero to 10 bar, and then barely moves. The melt temperature rises 26 degrees over the same range, and the last 20 bar buys 0.06 percent of consistency for 19 degrees of heat.<\/p>","protected":false},"author":1,"featured_media":8050,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[35],"tags":[],"class_list":["post-8052","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-injection-molding"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/8052","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/comments?post=8052"}],"version-history":[{"count":0,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/8052\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media\/8050"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media?parent=8052"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/categories?post=8052"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/tags?post=8052"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}