{"id":7662,"date":"2025-08-08T09:00:00","date_gmt":"2025-08-08T08:00:00","guid":{"rendered":"https:\/\/uplastech.com\/machining-acrylic-rod\/"},"modified":"2026-10-28T03:19:18","modified_gmt":"2026-10-28T03:19:18","slug":"machining-acrylic-rod","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ar\/machining-acrylic-rod\/","title":{"rendered":"Machining Acrylic Rod: Cutting, Drilling and Polishing Without Crazing"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}}\n\/* \u5355\u7bc7\u9875\u9690\u85cf WhatsApp \u81ea\u52a8\u5c55\u5f00\u7684\u95ee\u5019\u5361\uff0c\u53ea\u4fdd\u7559\u5706\u5f62\u6c14\u6ce1\uff0c\u907f\u514d\u906e\u6321\u4fa7\u680f\u8be2\u76d8\u63d0\u4ea4\u6309\u94ae *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure>\n<img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/10\/machining-acrylic-rod.jpg\" alt=\"Clear cast acrylic rod clamped on a lathe being turned with a sharp tool, producing a continuous transparent chip\" width=\"1536\" height=\"909\"><figcaption>Acrylic machines like a soft brass and cracks like glass. The difference between a clean turned surface and a crazed one is usually a few hundred rpm and one rake angle.<\/figcaption><\/figure>\n<div class=\"toc\"><\/div>\n<h2 id=\"character\">Acrylic is not a difficult material \u2014 it is an unforgiving one<\/h2>\n<p>Machinists who come from metal find acrylic easy: it cuts fast, it needs no coolant on most operations, and the surface finish can be optical. Machinists who come from other plastics find it frustrating, because the failure modes are delayed. A part that looks perfect on the bench can craze three weeks later, and the crack always starts where the tool was.<\/p>\n<p>The reason is that acrylic (PMMA) is amorphous and brittle. It has no crystalline phase to absorb energy, so any stress concentration stays concentrated. It is also notch-sensitive: a scratch, a tool mark or a sharp internal corner raises the local stress by a factor of three to five, and combined with residual stress from machining it is enough to propagate a crack.<\/p>\n<div class=\"callout\">\n<p><strong>The three rules that prevent most failures:<\/strong> keep the tool sharp, keep the feed high enough that the tool cuts rather than rubs, and anneal anything with a machined feature deeper than about 3 mm. Most acrylic failures are not caused by any one of these being wrong \u2014 they are caused by all three being slightly wrong at once.<\/p>\n<\/div>\n<h2 id=\"cutting\">Cutting to length<\/h2>\n<p>The first operation sets up everything downstream. A bad cut leaves a stressed, chipped end that will crack during the next operation or in service.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0627\u0644\u0637\u0631\u064a\u0642\u0629<\/th>\n<th>Edge quality<\/th>\n<th>Stress<\/th>\n<th>\u0627\u0644\u0623\u0641\u0636\u0644 \u0644\u0640<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Circular saw, carbide, triple-chip<\/td>\n<td>\u062c\u064a\u062f<\/td>\n<td>\u0645\u0646\u062e\u0641\u0636\u0629<\/td>\n<td>Production cutting of rod up to 100 mm<\/td>\n<\/tr>\n<tr>\n<td>Band saw, fine tooth<\/td>\n<td>Fair, needs finishing<\/td>\n<td>\u0645\u0646\u062e\u0641\u0636\u0629<\/td>\n<td>Large diameter, short runs<\/td>\n<\/tr>\n<tr>\n<td>Cold saw (low speed, flood coolant)<\/td>\n<td>\u0645\u0645\u062a\u0627\u0632<\/td>\n<td>Very low<\/td>\n<td>Precision blanks, large sections<\/td>\n<\/tr>\n<tr>\n<td>Laser cutting<\/td>\n<td>Polished edge<\/td>\n<td>High (heat affected)<\/td>\n<td>Thin sheet, not rod<\/td>\n<\/tr>\n<tr>\n<td>Waterjet<\/td>\n<td>Matt, no heat<\/td>\n<td>Very low<\/td>\n<td>Thick sections, complex profiles<\/td>\n<\/tr>\n<tr>\n<td>Tube cutter \/ score and snap<\/td>\n<td>\u0641\u0642\u064a\u0631<\/td>\n<td>\u0639\u0627\u0644\u064a\u0629<\/td>\n<td>Never on rod<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1 \u2014 Cutting methods for acrylic rod. Laser gives a beautiful edge and a stress field that cracks later; it is a sheet process, not a rod process.<\/p>\n<p>For a circular saw the parameters matter more than the blade. A triple-chip carbide blade with 60\u201380 teeth, running at 2,000\u20133,000 rpm with a feed of 0.05\u20130.1 mm per tooth, gives a clean edge. Too slow a feed and the blade rubs, generating heat and melting the surface; too fast and the teeth chip the exit edge.<\/p>\n<h2 id=\"turning\">\u0627\u0644\u062f\u0648\u0631\u0627\u0646<\/h2>\n<p>Turning is the most common operation on rod and the one where tool geometry decides the outcome. Acrylic needs a positive rake and a sharp edge \u2014 a tool that would be acceptable on aluminium will rub on acrylic and leave a dull, stressed surface.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0627\u0644\u0645\u0639\u0644\u0645\u0629<\/th>\n<th>Roughing<\/th>\n<th>\u0627\u0644\u062a\u0634\u0637\u064a\u0628<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Rake angle<\/td>\n<td>0 \u2013 5\u00b0 positive<\/td>\n<td>10 \u2013 15\u00b0 positive<\/td>\n<\/tr>\n<tr>\n<td>Clearance angle<\/td>\n<td>8 \u2013 10\u00b0<\/td>\n<td>10 \u2013 12\u00b0<\/td>\n<\/tr>\n<tr>\n<td>Spindle speed (\u00d825 mm)<\/td>\n<td>800 \u2013 1,200 rpm<\/td>\n<td>1,500 \u2013 2,500 rpm<\/td>\n<\/tr>\n<tr>\n<td>Feed<\/td>\n<td>0.15 \u2013 0.3 mm\/rev<\/td>\n<td>0.05 \u2013 0.1 mm\/rev<\/td>\n<\/tr>\n<tr>\n<td>Depth of cut<\/td>\n<td>1 \u2013 2 mm<\/td>\n<td>0.2 \u2013 0.5 mm<\/td>\n<\/tr>\n<tr>\n<td>Coolant<\/td>\n<td>Air blast or none<\/td>\n<td>Air blast; water mist for fine finish<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2 \u2014 Turning parameters for cast acrylic rod. The finishing pass should remove at least 0.2 mm, because a lighter pass rubs rather than cuts.<\/p>\n<p>The most common turning mistake is taking a very light finishing pass to \"be safe\". Below about 0.1 mm depth the tool tends to rub, which generates heat and work-hardens the surface layer into a stressed state. A 0.3 mm pass at higher speed gives a better surface and lower stress than a 0.05 mm pass.<\/p>\n<p>Tool material is usually high-speed steel or polished carbide. Carbide lasts longer but must be sharp \u2014 a worn carbide insert will rub and heat the surface. Diamond-tipped tools are used for optical work where the surface must be clear without polishing.<\/p>\n<h2 id=\"drilling\">\u0627\u0644\u062d\u0641\u0631<\/h2>\n<p>Drilling is where acrylic cracks most often, because the drill generates heat at the bottom of a hole it cannot escape from, and the flutes can grab and screw the bit into the material.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0627\u0644\u0645\u0639\u0644\u0645\u0629<\/th>\n<th>\u0627\u0644\u062a\u0648\u0635\u064a\u0629<\/th>\n<th>Reason<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Drill geometry<\/td>\n<td>90\u2013120\u00b0 point, slow spiral, relieved lands<\/td>\n<td>Standard 118\u00b0 jobber drills grab and chip<\/td>\n<\/tr>\n<tr>\n<td>Spindle speed<\/td>\n<td>500 \u2013 1,500 rpm (lower for large dia)<\/td>\n<td>Heat is the enemy; large drills need slower speed<\/td>\n<\/tr>\n<tr>\n<td>Feed<\/td>\n<td>0.05 \u2013 0.15 mm\/rev, steady<\/td>\n<td>Dwelling generates heat and melts<\/td>\n<\/tr>\n<tr>\n<td>Peck depth<\/td>\n<td>One diameter, then retract<\/td>\n<td>Clears chips and lets heat escape<\/td>\n<\/tr>\n<tr>\n<td>Coolant<\/td>\n<td>Compressed air, or water-soluble mist<\/td>\n<td>Air alone is often enough for shallow holes<\/td>\n<\/tr>\n<tr>\n<td>Backing<\/td>\n<td>Sacrificial backing on exit<\/td>\n<td>Prevents breakout and chipping<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3 \u2014 Drilling acrylic. The slow spiral and relieved lands are the two features that separate an acrylic drill from a general-purpose one.<\/p>\n<p>Deep holes are a separate problem. Beyond about three diameters, chips cannot clear and the drill overheats. The practical approach is to drill from both ends, or to use a coolant-fed drill. A deep hole that has been drilled hot will craze from the inside out over weeks, and there is no way to inspect for it.<\/p>\n<h2 id=\"polishing\">Polishing and the edge that has to be clear<\/h2>\n<p>Acrylic rod is usually bought for its clarity, so the machined surfaces have to be restored to transparency. That is a sequence, not a single step.<\/p>\n<table>\n<thead>\n<tr>\n<th>Stage<\/th>\n<th>Abrasive<\/th>\n<th>\u0627\u0644\u063a\u0631\u0636<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1. True the surface<\/td>\n<td>320 \u2013 400 grit wet<\/td>\n<td>Remove tool marks<\/td>\n<\/tr>\n<tr>\n<td>2. Refine<\/td>\n<td>600 \u2013 800 grit wet<\/td>\n<td>Remove previous scratches<\/td>\n<\/tr>\n<tr>\n<td>3. Fine<\/td>\n<td>1200 \u2013 1500 grit wet<\/td>\n<td>Surface becomes hazy<\/td>\n<\/tr>\n<tr>\n<td>4. Polish<\/td>\n<td>Aluminium oxide or cerium oxide slurry<\/td>\n<td>Removes haze<\/td>\n<\/tr>\n<tr>\n<td>5. Buff<\/td>\n<td>Cotton wheel with rouge or a plastic polish<\/td>\n<td>Optical clarity<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 4 \u2014 Polishing sequence. Every stage must remove the scratches of the previous one completely, or the final buff will reveal them.<\/p>\n<p>Flame polishing is faster and gives a glass-clear edge in seconds, but it introduces a heat-affected zone with high residual stress. On a rod that will be subject to load or thermal cycling, flame polishing is the starting point for later crazing. It is fine for display parts and decorative edges, and it is not fine for structural or outdoor use.<\/p>\n<h2 id=\"annealing\">Annealing: the step that is usually skipped<\/h2>\n<p>Machining leaves residual stress in acrylic. The stress is concentrated at the machined surface and at any sharp corner, and it is invisible. Annealing relaxes it, and it is the single most effective thing you can do to prevent delayed cracking.<\/p>\n<table>\n<thead>\n<tr>\n<th>Material thickness<\/th>\n<th>Annealing temperature<\/th>\n<th>Soak time<\/th>\n<th>Cooling rate<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Up to 6 mm<\/td>\n<td>80 \u00b0C<\/td>\n<td>1 hour<\/td>\n<td>10 \u00b0C\/hour<\/td>\n<\/tr>\n<tr>\n<td>6 \u2013 12 mm<\/td>\n<td>80 \u00b0C<\/td>\n<td>2 \u2013 3 hours<\/td>\n<td>8 \u00b0C\/hour<\/td>\n<\/tr>\n<tr>\n<td>12 \u2013 25 mm<\/td>\n<td>80 \u00b0C<\/td>\n<td>4 \u2013 6 hours<\/td>\n<td>6 \u00b0C\/hour<\/td>\n<\/tr>\n<tr>\n<td>25 \u2013 50 mm<\/td>\n<td>75 \u2013 80 \u00b0C<\/td>\n<td>8 \u2013 12 hours<\/td>\n<td>5 \u00b0C\/hour<\/td>\n<\/tr>\n<tr>\n<td>Over 50 mm<\/td>\n<td>70 \u2013 75 \u00b0C<\/td>\n<td>12 \u2013 24 hours<\/td>\n<td>3 \u2013 5 \u00b0C\/hour<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 5 \u2014 Annealing schedule for cast acrylic. The cooling rate matters as much as the soak \u2014 cooling too fast reintroduces the stress you just removed.<\/p>\n<p>The annealing temperature must stay below the point where the rod distorts. For cast acrylic that is around 80\u201385 \u00b0C; extruded acrylic softens lower and needs 70\u201375 \u00b0C. Above that the part will sag under its own weight, which on a long rod is visible as a bow.<\/p>\n<p>The test for whether annealing worked is a solvent test: wipe a machined surface with a solvent (isopropyl alcohol or a proper stress-crazing agent), let it evaporate, and look for fine cracks. An unannealed part will craze within seconds. An annealed part will not. It is a destructive test but it can be done on a test piece from the same batch.<\/p>\n<h2 id=\"troubleshooting\">Faults and causes<\/h2>\n<table>\n<thead>\n<tr>\n<th>Fault<\/th>\n<th>\u0627\u0644\u0645\u0638\u0647\u0631<\/th>\n<th>\u0627\u0644\u0633\u0628\u0628<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Crazing<\/td>\n<td>Fine cracks, often radiating from a machined edge<\/td>\n<td>Residual stress plus solvent or thermal cycling; no annealing<\/td>\n<\/tr>\n<tr>\n<td>Melted \/ gummy surface<\/td>\n<td>Smears, stringy chips<\/td>\n<td>Tool rubbing, too high rpm, dull tool, no chip clearance<\/td>\n<\/tr>\n<tr>\n<td>Chipping on exit<\/td>\n<td>Missing chunks at the far side of a hole or cut<\/td>\n<td>No backing support, too fast a feed at breakthrough<\/td>\n<\/tr>\n<tr>\n<td>Haze that will not polish out<\/td>\n<td>Persistent dull patch<\/td>\n<td>Heat damage from rubbing; material is degraded, must be machined deeper<\/td>\n<\/tr>\n<tr>\n<td>Bubbles appearing after machining<\/td>\n<td>Small voids near a machined surface<\/td>\n<td>Material had internal voids; machining exposed them<\/td>\n<\/tr>\n<tr>\n<td>Warping after machining<\/td>\n<td>Rod bends over days<\/td>\n<td>Asymmetric material removal releasing internal stress<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 6 \u2014 Machining faults in acrylic. Haze that will not polish out is not a polishing problem \u2014 the polymer has been thermally damaged and has to be cut away.<\/p>\n<p>Asymmetric removal is worth understanding on rod specifically. If you machine a flat on one side of a rod, you release stress on that side only, and the rod bends towards the cut. On cast rod the internal stress is usually low enough that this is minor; on extruded rod it can be significant. If the part needs a flat, machine small amounts from both sides in alternation where possible.<\/p>\n<h2 id=\"cast-vs-extruded\">Cast and extruded rod machine differently<\/h2>\n<p>The two production routes give different machining behaviour, and the difference is not always stated on the quote.<\/p>\n<p><strong>Cast rod<\/strong> has higher molecular weight, better optical clarity, lower internal stress and machines cleanly. It also costs more and comes in a narrower size range.<\/p>\n<p><strong>Extruded rod<\/strong> has lower molecular weight, slightly lower clarity, and higher internal stress \u2014 which means it is more prone to craze after machining and more prone to bend when material is removed asymmetrically. It is cheaper and available in continuous lengths.<\/p>\n<p>For a machined part with a critical clear surface or a tight tolerance, cast is the right choice. For a non-critical spacer or a decorative part, extruded is fine. The failure mode to watch for is specifying extruded to save money on a part that then crazes in service \u2014 the saving is a fraction of the part cost and the failure is total.<\/p>\n<div class=\"faq\">\n<h3>Why does acrylic crack weeks after machining?<\/h3>\n<p>Residual stress plus a stress raiser. Machining leaves stress in the surface, and any sharp corner, tool mark or scratch concentrates it. Add solvent exposure, thermal cycling or a load, and a crack propagates. Annealing at 80 \u00b0C after machining removes most of the risk.<\/p>\n<h3>Do I need coolant when machining acrylic?<\/h3>\n<p>Usually not for turning and milling, provided the tool is sharp and the chips clear. Compressed air is enough to keep the cut cool and clear chips. For drilling deep holes and for sawing thick sections, a water-soluble mist helps. Flood coolant is used on cold saws and is fine, but the parts must be dried properly.<\/p>\n<h3>What is the best way to drill a clean hole in acrylic rod?<\/h3>\n<p>Use a drill with a 90\u2013120\u00b0 point and slow spiral, run at 500\u20131,500 rpm depending on diameter, feed steadily at 0.05\u20130.15 mm\/rev, peck one diameter at a time to clear chips, and back the exit with a sacrificial piece. Never dwell \u2014 dwelling melts the material and creates a stress ring.<\/p>\n<h3>Can I flame polish acrylic rod?<\/h3>\n<p>Yes, for decorative edges. It gives a glass-clear finish in seconds. But it introduces a heat-affected zone with high residual stress, which is exactly the condition that leads to crazing later. Do not flame polish parts that will carry load, be exposed to solvents, or be used outdoors.<\/p>\n<h3>How long does acrylic need to be annealed?<\/h3>\n<p>Roughly one hour per 6 mm of thickness at 80 \u00b0C, then cool at 5\u201310 \u00b0C per hour. A 25 mm rod needs 4\u20136 hours soak and slow cooling. Cooling too fast reintroduces the stress, so the cooling ramp is as important as the soak time.<\/p>\n<h3>Why does my machined surface stay hazy no matter how much I polish?<\/h3>\n<p>Because the polymer has been thermally damaged, not just scratched. Rubbing tools generate enough heat to degrade the surface layer, and polishing removes material too slowly to get below it. The fix is to machine deeper with a sharp tool at a proper feed, then polish.<\/p>\n<h3>Does acrylic rod warp after machining?<\/h3>\n<p>Yes, if material is removed asymmetrically. Removing a flat from one side releases stress on that side only, and the rod bends towards the cut. Cast rod warps less than extruded. Machine from both sides in alternation where the geometry allows.<\/p>\n<h3>What is the difference between cast and extruded acrylic for machining?<\/h3>\n<p>Cast has higher molecular weight, better clarity, lower internal stress and machines more predictably. Extruded is cheaper and available in continuous lengths, but it crazes more readily and warps more when machined. For a clear, precise machined part, specify cast.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Need acrylic rod cut, machined or annealed to drawing?<\/p>\n<p>Send us the diameter, the grade (cast or extruded), the machined features and the clarity requirement. We will come back with a process route, the tolerance we can hold and whether annealing is needed for your application.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ar\/acrylic-rod\/\">Talk to an acrylic rod specialist<\/a>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ar\/acrylic-rod-specification-guide\/\">Acrylic Rod Sizes, Tolerances and Straightness<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/cast-vs-extruded-acrylic-rod\/\">Cast vs Extruded Acrylic Rod: Which One to Specify<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/acrylic-rod-defects\/\">Acrylic Rod Defects: Bubbles, Crazing and Colour Streaks<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/%d8%a8%d8%ab%d9%82-%d8%a7%d9%84%d8%a3%d9%86%d8%a7%d8%a8%d9%8a%d8%a8-%d9%88%d8%a7%d9%84%d8%a3%d9%86%d8%a7%d8%a8%d9%8a%d8%a8\/\">Plastic Pipe and Tube Extrusion: Materials and Sourcing<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/storing-handling-acrylic-rod\/\">Storing and Handling Acrylic Rod: Moisture, Film and Annealing<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Acrylic machines like a soft metal and cracks like glass. Tool geometry, feed rate, coolant and the annealing step that prevents crazing weeks later.<\/p>","protected":false},"author":1,"featured_media":7667,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_seopress_titles_title":"Machining Acrylic Rod: Cutting, Drilling and Polishing Witho","_seopress_titles_desc":"Acrylic machines like a soft metal and cracks like glass. Tool geometry, feed rate, coolant and the annealing step that prevents crazing weeks later.","_seopress_robots_index":"","_seopress_robots_follow":"","_seopress_robots_imageindex":"","_seopress_robots_snippet":"","_seopress_robots_primary_cat":"38","_seopress_robots_breadcrumbs":"","_seopress_robots_freeze_modified_date":"","_seopress_robots_custom_modified_date":"","_seopress_robots_canonical":"","_seopress_social_fb_title":"","_seopress_social_fb_desc":"","_seopress_social_fb_img":"","_seopress_social_fb_img_attachment_id":0,"_seopress_social_fb_img_width":0,"_seopress_social_fb_img_height":0,"_seopress_social_twitter_title":"","_seopress_social_twitter_desc":"","_seopress_social_twitter_img":"","_seopress_social_twitter_img_attachment_id":0,"_seopress_social_twitter_img_width":0,"_seopress_social_twitter_img_height":0,"_seopress_redirections_value":"","_seopress_redirections_enabled":"","_seopress_redirections_enabled_regex":"","_seopress_redirections_logged_status":"","_seopress_redirections_param":"","_seopress_redirections_type":0,"_seopress_analysis_target_kw":"machining acrylic rod","footnotes":""},"categories":[38],"tags":[],"class_list":["post-7662","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-acrylic-rod"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/7662","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/comments?post=7662"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/7662\/revisions"}],"predecessor-version":[{"id":7668,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/7662\/revisions\/7668"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media\/7667"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media?parent=7662"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/categories?post=7662"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/tags?post=7662"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}