{"id":10291,"date":"2026-11-18T01:00:00","date_gmt":"2026-11-18T01:00:00","guid":{"rendered":"https:\/\/uplastech.com\/?p=10291"},"modified":"2026-11-17T12:50:11","modified_gmt":"2026-11-17T12:50:11","slug":"injection-agricultural-pa-valve-splay-hydrolysis","status":"publish","type":"post","link":"https:\/\/uplastech.com\/ar\/injection-agricultural-pa-valve-splay-hydrolysis\/","title":{"rendered":"Silver Streaks on Nylon Irrigation Valves: Moisture, Not Dirt"},"content":{"rendered":"<style>\n.upl-blog{font-size:17px;line-height:1.78;color:#1f2937}\n.upl-blog p{margin:0 0 18px}\n.upl-blog h2{font-size:26px;line-height:1.3;color:#0b2b33;margin:46px 0 14px;font-weight:700;letter-spacing:-.015em}\n.upl-blog h3{font-size:19.5px;color:#0d3b47;margin:28px 0 10px;font-weight:700}\n.upl-blog ul,.upl-blog ol{margin:0 0 20px;padding-left:22px}\n.upl-blog li{margin:0 0 9px}\n.upl-blog figure{margin:0 0 34px}\n.upl-blog figure img{width:100%;height:auto;display:block;border-radius:10px}\n.upl-blog figcaption{font-size:13px;color:#6b7280;margin-top:10px;line-height:1.5}\n.upl-blog .toc{background:none;border:0;border-radius:0;padding:0;margin:0 0 34px}\n.upl-blog .toc .lwptoc{margin:0}\n.upl-blog .toc h4{margin:0 0 10px;font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#0d5563}\n.upl-blog .toc ol{margin:0;padding-left:18px;font-size:14.5px}\n.upl-blog .toc li{margin-bottom:6px}\n.upl-blog table{width:100%;border-collapse:collapse;font-size:14.5px;margin:0 0 10px}\n.upl-blog th{background:#0d3b47;color:#fff;text-align:left;padding:11px 13px;font-weight:600;font-size:13.5px;border:0}\n.upl-blog td{padding:11px 13px;border:0;border-bottom:1px solid #e8ebed;vertical-align:top}\n.upl-blog tbody tr:nth-child(even){background:#fafbfc}\n.upl-blog .tablecap{font-size:12.5px;color:#6b7280;margin:0 0 30px}\n.upl-blog .myth{background:#fff8ef;border:1px solid #f6ddbd;border-radius:8px;padding:16px 20px;margin:0 0 26px;font-size:15.5px}\n.upl-blog .myth b{color:#a85c10}\n.upl-blog .callout{background:#f2f8f9;border-radius:8px;padding:18px 22px;margin:0 0 26px;font-size:15.5px;border-left:3px solid #14707f}\n.upl-blog .faq h3{border-top:1px solid #eceff1;padding-top:22px;margin-top:0;font-size:18px}\n.upl-blog .faq h3:first-of-type{border-top:0;padding-top:0}\n.upl-blog .cta{background:linear-gradient(135deg,#0b2b33,#0d5563);color:#fff;border-radius:12px;padding:34px;margin:48px 0 30px}\n.upl-blog .cta h2,.upl-blog .cta .cta-h{color:#fff;margin:0 0 10px;font-size:24px;font-weight:700;line-height:1.3}\n.upl-blog .cta p{color:#c9dee3;margin:0 0 20px;font-size:16px}\n.upl-blog .btn{display:inline-block;background:#e07a1f;color:#fff;text-decoration:none;font-weight:700;padding:13px 26px;border-radius:8px;font-size:15.5px}\n.upl-blog .rel{border-top:1px solid #e8ebed;margin-top:40px;padding-top:26px}\n.upl-blog .rel h4{font-size:13px;letter-spacing:.1em;text-transform:uppercase;color:#6b7280;margin:0 0 14px}\n.upl-blog .rel ul{list-style:none;padding:0;margin:0}\n.upl-blog .rel li{padding:11px 0;border-bottom:1px dashed #e8ebed}\n.upl-blog .rel a{text-decoration:none;font-weight:600;font-size:15.5px}\n\/* ==UPL-CONVERSION-MODULES-START== 2024 problem-solving \/ lead-gen blocks *\/\n.upl-blog .mod-h{font-size:12.5px;letter-spacing:.12em;text-transform:uppercase;font-weight:700;color:#0d5563;margin:0 0 12px}\n.upl-blog .problem{background:#fff8f3;border:1px solid #f3ddc9;border-left:4px solid #e07a1f;border-radius:10px;padding:22px 26px;margin:0 0 32px;font-size:16px}\n.upl-blog .problem p{margin:0 0 10px}\n.upl-blog .problem p:last-child{margin-bottom:0}\n.upl-blog .problem .mod-h{color:#a85c10}\n.upl-blog .problem .problem-promise{font-weight:700;color:#0b2b33}\n.upl-blog .steps{background:#f7fafb;border:1px solid #e1ebee;border-radius:10px;padding:22px 26px;margin:0 0 28px}\n.upl-blog .steps ol{list-style:none;counter-reset:uplst;margin:0;padding:0}\n.upl-blog .steps li{counter-increment:uplst;position:relative;padding:0 0 16px 42px;margin:0;font-size:15.5px}\n.upl-blog .steps li:last-child{padding-bottom:0}\n.upl-blog .steps li::before{content:counter(uplst);position:absolute;left:0;top:2px;width:26px;height:26px;border-radius:50%;background:#0d5563;color:#fff;font-size:13px;font-weight:700;line-height:26px;text-align:center}\n.upl-blog table.spec th{background:#14707f}\n.upl-blog .conv{background:#eef6f7;border:1px solid #cfe4e8;border-radius:10px;padding:24px 26px;margin:32px 0}\n.upl-blog .conv p{margin:0 0 12px;font-size:15.5px}\n.upl-blog .conv .conv-lbl{font-weight:700;color:#0b2b33;margin:16px 0 8px}\n.upl-blog ul.conv-need{list-style:none;padding:0;margin:0 0 20px;display:grid;grid-template-columns:1fr 1fr;gap:6px 18px}\n.upl-blog ul.conv-need li{position:relative;padding-left:20px;margin:0;font-size:14.5px}\n.upl-blog ul.conv-need li::before{content:\"\";position:absolute;left:0;top:9px;width:9px;height:9px;border:2px solid #14707f;border-radius:2px}\n.upl-blog .conv-btn{display:inline-block;background:#0d5563;color:#fff;text-decoration:none;font-weight:700;padding:11px 22px;border-radius:7px;font-size:15px}\n.upl-blog .checklist{background:#fbfcfd;border:1px solid #e3e9ec;border-radius:10px;padding:24px 26px;margin:36px 0}\n.upl-blog .checklist ul{list-style:none;padding:0;margin:0 0 12px}\n.upl-blog .checklist li{position:relative;padding-left:28px;margin:0 0 10px;font-size:15.5px}\n.upl-blog .checklist li::before{content:\"\";position:absolute;left:0;top:7px;width:14px;height:14px;border:2px solid #0d5563;border-radius:3px}\n.upl-blog .cl-note{font-size:13.5px;color:#6b7280;margin:0}\n.upl-blog .cta .cta-lbl{color:#c9dee3;font-weight:700;margin:0 0 8px;font-size:14.5px}\n.upl-blog ul.cta-need{list-style:none;padding:0;margin:0 0 22px;display:grid;grid-template-columns:1fr 1fr;gap:4px 18px}\n.upl-blog ul.cta-need li{color:#e4f0f2;font-size:14.5px;padding-left:18px;position:relative;margin:0}\n.upl-blog ul.cta-need li::before{content:\"\\2713\";position:absolute;left:0;color:#e07a1f;font-weight:700}\n\/* ==UPL-CONVERSION-MODULES-END== *\/\n@media(max-width:640px){.upl-blog h2{font-size:22px}.upl-blog table{font-size:13px}.upl-blog .cta{padding:24px}.upl-blog ul.conv-need,.upl-blog ul.cta-need{grid-template-columns:1fr}.upl-blog .problem,.upl-blog .steps,.upl-blog .conv,.upl-blog .checklist{padding:18px}}\n\/* Single-post: hide the greeting card, keep the round WhatsApp bubble.\n   The Click to Chat logic refuses to open a chat while the greeting node exists,\n   so Code Snippets #9 removes that node from the DOM. This rule is only the visual fallback.\n   Delete #9 before removing this rule. *\/\nbody.single-post .ht_ctc_chat_greetings_box{display:none !important}\n<\/style>\n<div class=\"upl-blog\">\n<figure><img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/2024-injection-molding-sample-approval-to-production-hero.jpg\" alt=\"Silver Streaks on Nylon Irrigation Valves: Moisture, Not Dirt\" \/><figcaption>Injection moulding: a production part is the only useful reference for a discussion about process drift.<\/figcaption><\/figure>\n<p class=\"lead\">Pale splay streaks fan out from the gate on nylon valve bodies and the parts fail a pressure test, despite clean-looking granules.<\/p>\n<div class=\"toc\"><\/div>\n<h2 id=\"what\">What the failure looks like on the line<\/h2>\n<p>Agricultural mouldings live outdoors, see fertiliser and wash-down chemicals, and are judged a season later rather than on the day they are moulded.<\/p>\n<p>Silvery streaks radiate along the flow from the gate on moulded polyamide valve bodies. The same parts show reduced pressure retention and the granule bags feel slightly damp.<\/p>\n<p>Polyamide is hygroscopic; residual moisture flashes to steam at injection temperature and hydrolyses the melt, shortening chains and leaving gas streaks along the flow front. The hydrolysis lowers molecular weight, so the part loses ductility and pressure retention even where the surface mark is faint. A dryer with a poor dew point or long open hopper time re-wets the resin between drying and moulding.<\/p>\n<p>Buyers and suppliers usually agree on the drawing and disagree on the conditions under which the drawing was checked. On a buyer's specification this distinction matters: a part can measure inside tolerance and still fail in use, because the drawing records geometry while the complaint records behaviour. Resin moisture at the hopper is usually the first value both sides compare, and it is also the one most often quoted without the conditions attached to it.<\/p>\n<h2 id=\"window\">The process window that decides it<\/h2>\n<p>Four variables move this result more than the rest. The ranges below are illustrative engineering guidance for a first discussion; confirm them on your own tool, material grade and part geometry before they become contract terms.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0645\u062a\u063a\u064a\u0631<\/th>\n<th>Typical window<\/th>\n<th>What fails outside it<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Resin moisture at the hopper<\/td>\n<td>&lt; 0.2 % by mass<\/td>\n<td>Above the window hydrolysis produces splay and chain loss<\/td>\n<\/tr>\n<tr>\n<td>Dryer dew point<\/td>\n<td>-20 to -40 C<\/td>\n<td>A warm dew point cannot pull moisture below the limit<\/td>\n<\/tr>\n<tr>\n<td>Drying time<\/td>\n<td>4-8 h at 80 C<\/td>\n<td>Short drying leaves core moisture in the granule<\/td>\n<\/tr>\n<tr>\n<td>Hopper residence after drying<\/td>\n<td>&lt; 1 h<\/td>\n<td>Long open exposure re-wets the dried resin<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 1. Starting window for a joint process trial. Values are engineering guidance, not a measured survey.<\/p>\n<p><b>Resin moisture at the hopper<\/b> is typically held at &lt; 0.2 % by mass. Above the window hydrolysis produces splay and chain loss Record it together with the measurement point and the moment in the cycle; a single number without a location is not a process setting.<\/p>\n<p><b>Dryer dew point<\/b> is typically held at -20 to -40 C. A warm dew point cannot pull moisture below the limit When this drifts, the symptom usually appears at one cavity, one sheet position or one lane before it appears across the whole batch.<\/p>\n<p><b>Drying time<\/b> is typically held at 4-8 h at 80 C. Short drying leaves core moisture in the granule A change here is cheap during a trial and expensive after tooling release, so treat it as a controlled variable with a documented re-approval.<\/p>\n<p><b>Hopper residence after drying<\/b> is typically held at &lt; 1 h. Long open exposure re-wets the dried resin Put it on the change-control list, otherwise an unannounced material or setting substitution will be mistaken for ordinary process noise.<\/p>\n<h2 id=\"response\">Reading the response curve<\/h2>\n<figure><img decoding=\"async\" src=\"https:\/\/uplastech.com\/wp-content\/uploads\/2026\/11\/injection-agricultural-pa-valve-splay-hydrolysis-chart.jpg\" alt=\"Silver Streaks on Nylon Irrigation Valves: Moisture, Not Dirt: Pressure retention (%) against Drying time (h)\" \/><figcaption>Figure 1. Left: Pressure retention (%) against Drying time (h). Right: how audited failures of this type typically split by cause. All plotted values are illustrative engineering guidance, not a measured survey.<\/figcaption><\/figure>\n<p>The left panel shows pressure retention (%) as drying time (h) increases: the response rises from 30 to 95 on the illustrative 0&ndash;100 scale. The dashed line at 60 marks a proposed acceptance limit, not a universal standard. Move that line only after the test method and the sample plan have been agreed, otherwise two suppliers can both be compliant and still deliver different parts.<\/p>\n<p>Read the shape rather than a single point. A curve that changes quickly near the limit is more sensitive to ordinary process noise than one that approaches it gradually, and that difference should be reflected in how tightly the setting is controlled and how often it is checked.<\/p>\n<h2 id=\"causes\">Where the causes actually sit<\/h2>\n<p>The right panel of Figure 1 splits audited failures of this type into five groups. The percentages are illustrative engineering guidance for prioritising an investigation, not a measured survey and not a prediction for your line.<\/p>\n<table>\n<thead>\n<tr>\n<th>\u0627\u0644\u0633\u0628\u0628<\/th>\n<th>Illustrative share<\/th>\n<th>First check<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Wet resin at the hopper<\/td>\n<td>36%<\/td>\n<td>Measure moisture at the machine hopper, not only at the dryer outlet.<\/td>\n<\/tr>\n<tr>\n<td>Poor dryer dew point<\/td>\n<td>24%<\/td>\n<td>Log the dryer dew point and the open-hopper time for the affected lot.<\/td>\n<\/tr>\n<tr>\n<td>Long open-hopper re-wetting<\/td>\n<td>18%<\/td>\n<td>Compare a part moulded from freshly dried resin against the suspect lot.<\/td>\n<\/tr>\n<tr>\n<td>Short drying time<\/td>\n<td>14%<\/td>\n<td>Section a streaked wall and check for a spongy, hydrolysed core.<\/td>\n<\/tr>\n<tr>\n<td>High melt temperature driving hydrolysis<\/td>\n<td>8%<\/td>\n<td>Re-test pressure retention after a controlled re-dry of the resin.<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 2. Cause split and the corresponding first check. Shares are indicative and sum to 100.<\/p>\n<p><b>Wet resin at the hopper<\/b> accounts for roughly 36% of the illustrative split. Measure moisture at the machine hopper, not only at the dryer outlet. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.<\/p>\n<p><b>Poor dryer dew point<\/b> accounts for roughly 24% of the illustrative split. Log the dryer dew point and the open-hopper time for the affected lot. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.<\/p>\n<p><b>Long open-hopper re-wetting<\/b> accounts for roughly 18% of the illustrative split. Compare a part moulded from freshly dried resin against the suspect lot. Start here before authorising a material or tooling change, because it is the fastest explanation to confirm or eliminate.<\/p>\n<h2 id=\"checks\">Checks before sign-off<\/h2>\n<p>Run the same sequence on a retained good sample and on the disputed batch so the comparison means something.<\/p>\n<ol>\n<li>Measure moisture at the machine hopper, not only at the dryer outlet.<\/li>\n<li>Log the dryer dew point and the open-hopper time for the affected lot.<\/li>\n<li>Compare a part moulded from freshly dried resin against the suspect lot.<\/li>\n<li>Section a streaked wall and check for a spongy, hydrolysed core.<\/li>\n<li>Re-test pressure retention after a controlled re-dry of the resin.<\/li>\n<\/ol>\n<p>Keep a retained reference sample beside every result. When a batch is disputed, the comparison that settles it is almost always between the retained part and the current one under the same method, not between either part and a number on a drawing. Record the instrument, the operator, the conditioning time and the position on the part or sheet for each reading.<\/p>\n<h2 id=\"specification\">Writing it into the specification and the evidence pack<\/h2>\n<p>Resin moisture shall be recorded at the hopper before start-up and a first-off part checked for splay against an agreed limit sample; parts showing streaks or falling below the agreed pressure-retention limit are rejectable, with the moisture limit verified rather than assumed.<\/p>\n<p>Write the requirement as a behaviour at a stated condition, not as a brand of material or a machine setting. State the test method, the conditioning, the sample plan and the rule for deciding a pass. Where a document is needed, ask the supplier for documentation that covers the actual construction and check its scope against your own market before approval; a document for the base material alone does not describe the finished part you are buying.<\/p>\n<p>At first-article approval, freeze the drawing revision, the material and colour identification, the process window, the tool and cavity identification, and the inspection method. Any later change to grade, site, tool, or window should trigger a new first article rather than a paper waiver. Keep retained samples from the approved lot and from each production lot so that a future comparison is possible.<\/p>\n<table>\n<thead>\n<tr>\n<th>Evidence item<\/th>\n<th>What it must show<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Approved drawing and revision<\/td>\n<td>The exact geometry and tolerances the decision applies to<\/td>\n<\/tr>\n<tr>\n<td>Material and colour identification<\/td>\n<td>Grade, supplier, colour reference and any declared recycled content<\/td>\n<\/tr>\n<tr>\n<td>Process window and change log<\/td>\n<td>The agreed settings and any deviation since approval<\/td>\n<\/tr>\n<tr>\n<td>Inspection record and retained samples<\/td>\n<td>Method, conditions, results and a physical reference from the same lot<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"tablecap\">Table 3. Minimum evidence pack for a first-article decision and a later batch dispute.<\/p>\n<p>All ranges in this article are illustrative engineering guidance rather than measured data. Treat them as a starting agenda for a process trial, not as a certificate for a batch that has not been run.<\/p>\n<div class=\"faq\">\n<h2 id=\"questions\">Questions buyers ask<\/h2>\n<h3>Is this a material problem or a process problem?<\/h3>\n<p>Polyamide is hygroscopic; residual moisture flashes to steam at injection temperature and hydrolyses the melt, shortening chains and leaving gas streaks along the flow front. The hydrolysis lowers molecular weight, so the part loses ductility and pressure retention even where the surface mark is faint. A dryer with a poor dew point or long open hopper time re-wets the resin between drying and moulding. It is worth separating the two before a supplier changes a grade: hold the material constant for one controlled run, then move one setting at a time. If the symptom follows the setting, the material was never the cause.<\/p>\n<h3>Can resin moisture at the hopper be traded against cycle time?<\/h3>\n<p>Only within the window stated in Table 1, and only with a recorded trial. Above the window hydrolysis produces splay and chain loss A faster cycle that sits outside the window usually moves the failure downstream, where it costs more to find.<\/p>\n<h3>What should be recorded at incoming inspection?<\/h3>\n<p>Keep the measurement, the method, the sample identity and the conditions together. Measure moisture at the machine hopper, not only at the dryer outlet. A result without its conditions cannot be compared with a later batch.<\/p>\n<h3>Does a change of agricultural require re-approval?<\/h3>\n<p>Treat any change to material grade, tool, site or process window as a change that needs a new first-article decision. For injection moulding work the drawing alone is not enough; the process route is part of what was approved.<\/p>\n<h3>How many samples are enough for a first-article decision?<\/h3>\n<p>There is no universal number. Sample across cavities, lanes, sheet positions or reel lengths so that the spread is visible, not just the average. Agree the sample plan and the acceptance rule with the supplier before the trial starts.<\/p>\n<h3>What belongs in the evidence pack?<\/h3>\n<p>The approved drawing and revision, the material and colour identification, the process window, the inspection method and results, the retained reference samples, and documentation covering the actual construction. Ask the supplier to state the scope of each document and check it against your own market.<\/p>\n<\/div>\n<div class=\"cta\">\n<p class=\"cta-h\">Seeing this on a current injection moulding job?<\/p>\n<p>Send the drawing, the material and grade, the process window you are running, and the point in the cycle or the shelf life where the fault appears. We will help you separate a material question from a process question and a specification question before anyone changes a tool.<\/p>\n<p><a class=\"btn\" href=\"https:\/\/uplastech.com\/ar\/%d8%a7%d9%84%d8%a7%d8%aa%d8%b5%d8%a7%d9%84\/\">Talk to our injection moulding team<\/a><\/p>\n<\/div>\n<div class=\"rel\">\n<h4>Continue reading<\/h4>\n<ul>\n<li><a href=\"https:\/\/uplastech.com\/ar\/silver-streak-moisture\/\">Silver Streaks and Splay: Moisture, Shear and the Dryer That Lies<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/resin-dryer-dew-point-audit-moulding-quote\/\">Resin Dryer Dew Point: Splay and the Supply Contract<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/nylon-pa-injection-molding-guide\/\">Nylon (PA6 \/ PA66) Injection Molding: Moisture, Conditioning and Dimensions<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/plastic-drying-before-extrusion\/\">Plastic Drying Before Extrusion: Hygroscopic vs Non-Hygroscopic Resins<\/a><\/li>\n<li><a href=\"https:\/\/uplastech.com\/ar\/injection-molding-material-selection\/\">Injection Molding Material Selection: 14 Plastics Compared<\/a><\/li>\n<\/ul>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Pale splay streaks fan out from the gate on nylon valve bodies and the parts fail a pressure test, despite clean-looking granules.<\/p>","protected":false},"author":1,"featured_media":9862,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[35],"tags":[],"class_list":["post-10291","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-injection-molding"],"meta_box":{"post-to-quiz_to":[]},"_links":{"self":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/10291","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/comments?post=10291"}],"version-history":[{"count":1,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/10291\/revisions"}],"predecessor-version":[{"id":11997,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/posts\/10291\/revisions\/11997"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media\/9862"}],"wp:attachment":[{"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/media?parent=10291"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/categories?post=10291"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uplastech.com\/ar\/wp-json\/wp\/v2\/tags?post=10291"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}